MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes HR-120® alloy, solution heat-treated
Categories: Metal; Superalloy; Iron Base

Material Notes: Excellent strength at elevated temperatures, combined with good resistance to carburizing and sulfidizing environments. Applications include bar frame heat treating baskets, wire mesh furnace belts and basket liners, muffles and retorts, heat treating fixtures, waste incinerators, radiant tubes, cast link belt pins, recuperators, and fluidized bed components.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: ASTM B514, ASTM B407, ASTM B515, ASTM B564, ASTM B366, DIN No.2.4854, UNS N08120, ASTM B163, ASTM B408, ASTM B409
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.07 g/ccat RT.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 735 MPa
Tensile Strength, Yield 375 MPa
@Strain 0.2 %
Elongation at Break 50 %in 1.4 inches
Modulus of Elasticity 197 GPaRT
 128 GPa
@Temperature 1000 °C
 136 GPa
@Temperature 900 °C
 143 GPa
@Temperature 800 °C
 152 GPa
@Temperature 700 °C
 159 GPa
@Temperature 600 °C
 165 GPa
@Temperature 500 °C
 174 GPa
@Temperature 400 °C
 182 GPa
@Temperature 300 °C
 188 GPa
@Temperature 200 °C
 194 GPa
@Temperature 100 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0001052 ohm-cmRT
 0.0001231 ohm-cm
@Temperature 700 °C
 0.0001245 ohm-cm
@Temperature 800 °C
 0.0001257 ohm-cm
@Temperature 900 °C
 0.0001266 ohm-cm
@Temperature 1000 °C
 0.0001278 ohm-cm
@Temperature 1100 °C
 0.0001287 ohm-cm
@Temperature 1200 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.3 µm/m-°C
@Temperature 25.0 - 100 °C
 14.9 µm/m-°C
@Temperature 25.0 - 200 °C
 15.3 µm/m-°C
@Temperature 25.0 - 300 °C
 15.8 µm/m-°C
@Temperature 25.0 - 400 °C
 16.1 µm/m-°C
@Temperature 25.0 - 500 °C
 16.4 µm/m-°C
@Temperature 25.0 - 600 °C
 16.9 µm/m-°C
@Temperature 25.0 - 700 °C
 17.3 µm/m-°C
@Temperature 25.0 - 800 °C
 17.6 µm/m-°C
@Temperature 25.0 - 900 °C
 17.8 µm/m-°C
@Temperature 25.0 - 1000 °C
Specific Heat Capacity 0.467 J/g-°CRT
 0.483 J/g-°C
@Temperature 100 °C
 0.500 J/g-°C
@Temperature 200 °C
 0.522 J/g-°C
@Temperature 300 °C
 0.531 J/g-°C
@Temperature 400 °C
 0.558 J/g-°C
@Temperature 500 °C
 0.607 J/g-°C
@Temperature 600 °C
 0.647 J/g-°C
@Temperature 700 °C
 0.655 J/g-°C
@Temperature 800 °C
 0.660 J/g-°C
@Temperature 900 °C
 0.663 J/g-°C
@Temperature 1000 °C
 0.667 J/g-°C
@Temperature 1100 °C
 0.671 J/g-°C
@Temperature 1200 °C
Thermal Conductivity 11.4 W/m-KRT
 12.6 W/m-K
@Temperature 100 °C
 14.3 W/m-K
@Temperature 200 °C
 15.9 W/m-K
@Temperature 300 °C
 17.5 W/m-K
@Temperature 400 °C
 19.0 W/m-K
@Temperature 500 °C
 20.6 W/m-K
@Temperature 600 °C
 22.2 W/m-K
@Temperature 700 °C
 23.8 W/m-K
@Temperature 800 °C
 25.4 W/m-K
@Temperature 900 °C
 27.1 W/m-K
@Temperature 1000 °C
Melting Point 1300 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.10 %
Boron, B 0.0040 %
Carbon, C 0.050 %
Chromium, Cr 25 %
Cobalt, Co <= 3.0 %
Iron, Fe 33 %
Manganese, Mn 0.70 %
Molybdenum, Mo <= 2.5 %
Nickel, Ni 37 %
Niobium, Nb (Columbium, Cb) 0.70 %
Nitrogen, N 0.20 %
Silicon, Si 0.60 %
Tungsten, W <= 2.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
MetalTek HAYNES® HR120 Severe Corrosion and Heat Resistant Alloy
ATI Allvac® Rene 41® Nickel Superalloy, Heat Treatment: 1079°C (1975°F) + Age
Rene 100 Nickel Alloy (UNS N13100)
Rene 85 Nickel Superalloy
Special Metals NIMONIC® Alloy 80A

NH120I / 16318

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.