MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Kingfa LONOY 6100 Flame Retardant PC/PBT Alloy
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Unreinforced; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes:
    Features:
  • Excellent balance properties
  • Good weather resistance
  • Good size stability
  • Smooth surface
  • Uniform color

    Applications:
  • Injection molding
  • Electric and electronic parts
  • Business machine cabinet
  • Garden tools
  • OA device and parts

Information Provided by Kingfa Sci. & Tech. Co., Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.24 g/cc
@Temperature 23.0 °C
1.24 g/cc
@Temperature 73.4 °F
ASTM D792
Water Absorption 0.10 %
@Temperature 23.0 °C,
Time 86400 sec
0.10 %
@Temperature 73.4 °F,
Time 24.0 hour
ASTM D570
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm
@Temperature 23.0 °C
0.0040 - 0.0070 in/in
@Temperature 73.4 °F
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 9595ASTM D785
Tensile Strength at Break 56.0 MPa8120 psi50mm/min; ASTM D638
Elongation at Break 100 %100 %50mm/min; ASTM D638
Flexural Strength 85.0 MPa12300 psi2mm/min; ASTM D790
Flexural Modulus 2.30 GPa334 ksi2mm/min; ASTM D790
Izod Impact, Notched >= 7.00 J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
>= 13.1 ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
Izod Impact, Unnotched NB
@Thickness 3.20 mm,
Temperature 23.0 °C
NB
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmASTM D257
Surface Resistance 1.00e+12 ohm1.00e+12 ohmASTM D257
Dielectric Strength 30.0 kV/mm762 kV/in1.6mm; ASTM D149
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 110 °C
@Thickness 6.40 mm
230 °F
@Thickness 0.252 in
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 100 °C
@Thickness 6.40 mm
212 °F
@Thickness 0.252 in
ASTM D648
Flammability, UL94 V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature <= 280 °C<= 536 °F
Rear Barrel Temperature 245 - 260 °C473 - 500 °FStart Point: 250°C
Middle Barrel Temperature 250 - 270 °C482 - 518 °FStart Point: 255°C
Front Barrel Temperature 250 - 270 °C482 - 518 °FStart Point: 260°C
Melt Temperature 245 - 270 °C473 - 518 °FStart Point: 260°C
Mold Temperature 70.0 - 90.0 °C158 - 194 °FStart Point: 80°C
Drying Temperature 120 °C
@Time 14400 - 21600 sec
248 °F
@Time 4.00 - 6.00 hour
Pre-dry
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
 
Descriptive Properties
Injection Speed60-100%

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kingfa LONOY 1600 PC/PBT Alloy
Teijin Multilon TN-7500 Halogen-Free Flame Resistant PC/ABS Polymer Alloy
Kingfa LONOY 1200 PC/PBT Alloy
Loxim 200 00V0 Polybutylene Terephthalate
Star Plastics PC/PBTQX7008 Molding Grade PC/PBT

PKINGF086 / 104345

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.