MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Mateck Laser Grade Zinc Selenide, ZnSe CVD
Categories: Ceramic; Sulfide/Chalcogenide; Other Engineering Material; Semiconductor

Material Notes: Optical Crystals

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 5.27 g/cc
@Temperature 20.0 °C
Solubility 0.00 ppm
Molecular Weight 144.33 g/mol
 
Mechanical PropertiesOriginal ValueComments
Vickers Microhardness 820MPa
Hardness, Mohs 4.0
Modulus of Elasticity 70.3 GPa
Poissons Ratio 0.28
Shear Modulus 27.5 GPaCalculated
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.57 µm/m-°C
Specific Heat Capacity 0.339 J/g-°C
Thermal Conductivity 16.0 W/m-K
@Temperature 20.0 °C
 
Optical PropertiesOriginal ValueComments
Refractive Index 2.4028at n10.6
 2.3448
@Wavelength 17000 nm
 2.4295
@Wavelength 5000 nm
 2.4892
@Wavelength 1000 nm
 2.6754
@Wavelength 580 nm
 
Descriptive Properties
Symmetrycubic
Symmetry Class43m
Thermal Coefficient of Refractive Index6.1E-05
Transmission Range (microns)0.55 - 20

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mateck Window Grade Zinc Selenide, ZnSe
Zinc Selenide, ZnSe
Mateck Zinc Selenide, ZnSe
MarkeTech Zinc Selenide:Tellurium (ZnSe:Te) Scintillator Crystal
Mateck Zinc Sulfide Cleartran (ZnS)

CMAT057 / 87741

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.