MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Envalior Pocan® S 7926 000000 PBT
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Flame Retardant

Material Notes: PBT, Improved toughness, flame retardant

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.37 g/cc0.0495 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.021 cm/cm0.021 in/inPlaque 60 x 60 x 2mm; ISO 294-4
Linear Mold Shrinkage, Transverse 0.020 cm/cm0.020 in/inPlaque 60 x 60 x 2mm; ISO 294-4
Melt Flow 40 g/10 min
@Load 5.00 kg,
Temperature 270 °C
40 g/10 min
@Load 11.0 lb,
Temperature 518 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 40.0 MPa5800 psi50 mm/min; ISO 527-1,-2
Elongation at Break >= 10 %>= 10 %Nominal, 50 mm/min; ISO 527-1,-2
Elongation at Yield 3.0 %3.0 %50 mm/min; ISO 527-1,-2
Tensile Modulus 2.40 GPa348 ksi1 mm/min; ISO 527-1,-2
Flexural Yield Strength 65.0 MPa
@Strain 3.5 %
9430 psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Strain at Yield 5.0 %5.0 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)  <= 10.0 kJ/m²
@Temperature 23.0 °C
<= 4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
<= 4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
Izod Impact, Unnotched (ISO)  110 kJ/m²
@Temperature -30.0 °C
52.3 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1U
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 180-1U
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179-1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179-1eU
Charpy Impact, Notched  <= 1.00 J/cm²
@Temperature -30.0 °C
<= 4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eA
 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.1
@Frequency 1e+6 Hz
3.1
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.024
@Frequency 1e+6 Hz
0.024
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VTest solution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C
@Temperature 23.0 - 55.0 °C
61.1 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
66.7 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 60.0 °C140 °FMethod Af; ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 130 °C266 °FMethod Bf; ISO 75-1,-2
Flammability, UL94  V-2
@Thickness 0.380 mm
V-2
@Thickness 0.0150 in
UL Yellow Card
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
UL Yellow Card
 5VB
@Thickness 1.50 mm
5VB
@Thickness 0.0591 in
UL Yellow Card
 5VA
@Thickness 3.00 mm
5VA
@Thickness 0.118 in
UL Yellow Card
Glow Wire Ignition Temperature 775 °C
@Thickness 0.750 mm
1430 °F
@Thickness 0.0295 in
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.750 mm
1760 °F
@Thickness 0.0295 in
IEC 60695-2-12
Shrinkage, MD 0.30 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.30 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Flow Direction Post-Molding, Plaque 60 x 60 x 2mm; ISO 294-4
Shrinkage, TD 0.30 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.30 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Post-Molding, Plaque 60 x 60 x 2mm; ISO 294-4
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 °C482 °FPlaque 60 x 60 x 2mm
Mold Temperature 80.0 °C176 °FPlaque 60 x 60 x 2mm
Hold Pressure 60.0 MPa8700 psiPlaque 60 x 60 x 2mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CP-Polymer-Technik Wellamid® 6600 PA-66-HWV0CP UL-Licensed Nylon 66, Flame Protection, Heat Stabilized, Dry
Eurotec® Tecolen® CP30 NL XA80 PPCP, flame retardant - halogen (RoHS compliant), heat stabilized, natural
Envalior Pocan® TS 3221 901510 PBT+PET, 20% Glass Fiber Reinforced
Envalior Pocan® S 7020 000000 PBT
Envalior Pocan® C 1202 000000 PBT+PC

PLANW9047 / 208462

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.