MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Total 3802 Blue MDPE pipe, injection molding
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Pipe Grade

Material Notes: FINATHENE® 3802 Blue is a polyethylene copolymer based on C6 hexene as co-monomer and is produced by a continuous low pressure slurry polymerization process.

FINATHENE® 3802 Blue is a blue polyethylene specially developed for the manufacture of pressure pipes and fittings. Its well balanced property profile and composition makes FINATHENE® 3802 Blue perfectly suited for potable water distribution.

Information provided provided by Total Petrochemicals.

Total Petrochemicals acquired former Fina and Atofina plastics product lines.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.941 g/ccASTM D 792
Viscosity 1.30e+6 cP
@Shear Rate 100 1/s,
Temperature 190 °C
ATOFINA research test
Environmental Stress Crack Resistance >= 700 hourASTM D1693
Oxidative Induction Time (OIT) >= 20 min210°C; EN 728
 >= 30 min200°C; EN 728
Melt Flow 0.20 g/10 min
@Load 2.16 kg
ASTM D 1238
 0.92 g/10 min
@Load 5.00 kg
ASTM D 1238
High Load Melt Index 18 g/10 min
@Load 21.6 kg
ASTM D 1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 32.0 MPaISO 527
Tensile Strength, Yield 18.0 MPaISO 527
Elongation at Break >= 700 %ISO R527
Elongation at Yield 9.0 %ISO 527
Modulus of Elasticity 0.700 GPaISO 178
Flexural Modulus 0.700 GPaASTM D 790
Charpy Impact, Notched >= 1.00 J/cm²
@Temperature 23.0 °C
ISO 170
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+17 ohm-cmIEC 93
Surface Resistance >= 1.00e+16 ohmIEC 93
Dielectric Constant 2.45
@Frequency 1000 Hz
IEC 250
Dielectric Strength 16.0 kV/mmIEC 243
Dissipation Factor 0.020
@Frequency 1000 Hz
IEC 250
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 161 J/gDSC
CTE, linear 120 µm/m-°C
@Temperature 20.0 °C
Specific Heat Capacity 2.00 J/g-°CDSC
 2.60 J/g-°C
@Temperature 150 °C
DSC
Thermal Conductivity 0.400 W/m-KDIN 52612
 0.200 W/m-K
@Temperature 150 °C
DIN 52612
Melting Point 125 - 129 °Ccrystalline; DSC
Vicat Softening Point 125 °CISO 306
Brittleness Temperature -100 °CASTM D 746

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Petromont 2100 Medium Density Polyethylene Resin
Chevron Phillips HiD® 9300 HDPE Orange Pipe Resin
Chevron Phillips Marlex® HP076 High Density Polyethylene, Pipe Grade
Entec Hypel® PEHD.3/.955 HDPE
LyondellBasell Alathon L 4930TC High Denisty Polyethylene

PFINAP111 / 38694

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.