MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Marco Polo MARPOL EVA 802 EVA
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: MARPOL® EVA 802 is an 8.7% vinyl acetate copolymer film resin with excellent impact strength and heat sealability.

Recommended Applications: Films for meat packaging and primal meat bags, heavy-duty bags.

Additives: Antiblock – no, Slip – no.

Processing Notes: Melt temperatures of 360°F – 390°F (182 °C - 200 °C) are recommended for this resin. This resin grade complies with 21 CFR 177.1350.

Information provided by Marco Polo International, LLC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.930 g/cc0.0336 lb/in³ASTM D1505
Vinyl Acetate Content 8.7 %8.7 %
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 330 %330 %ASTM D882
Film Elongation at Break, TD 660 %660 %ASTM D882
Flexural Modulus, 1% Secant 110 MPa16000 psiMD; ASTM D882
 117 MPa17000 psiTD; ASTM D882
Tear Strength Test 250250[g], Elmendorf; ASTM D 1922
Dart Drop Test 250 g0.551 lbASTM D1709
Film Tensile Strength at Break, MD 30.3 MPa4400 psiASTM D882
Film Tensile Strength at Break, TD 27.6 MPa4000 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 81.0 °C178 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 1.5 %1.5 %ASTM D1003
Gloss 88 %88 %45°; ASTM D2457
 
Processing PropertiesMetricEnglishComments
Melt Temperature 182 - 200 °C360 - 392 °F
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PMARCO205 / 283802

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.