MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Toyobo Celstran® PA66-GF50-01 Nylon 66/6, 50% Long Glass Reinforced, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, 40% Glass Fiber Reinforced

Material Notes: Product Description: Material code according to ISO 1043-1: PA66 Nylong 66 reinforced by 50% long glass fibers. The pellets are cylindrical and normally as well as the embedded fibers 10mm long. Parts molded of CELSTRAN have outstanding mechanical properties such as high strength and stiffness combined with high heat deflection. The notched impact strength is increased at elevated and low temperatures due to the fiber skeleton build in the parts. The long fiber reinforcement reduces creep significantly. The very isotropic shrinkage in the molded parts minimizes the warpage. Complex parts can be manufactured with high reproducibility by injection molding. Can be used for substituting die cast metal with the advantage of weight reduction, no corrosion problems, no post treatment.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Filler/Reinforcement: Glass Fiber

Forms: Pellets

Processing Method: Injection Molding

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.56 g/ccISO 1183
Maximum Moisture Content 0.15
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 25400 psiISO 527-2/5
Elongation at Break 2.4 %ISO 527-2/5
Tensile Modulus 1.62e+6 psiISO 527-1
Flexural Strength 30500 psi
@Temperature 80.0 °C
ISO 178
 37700 psi
@Temperature 22.8 °C
ISO 178
Flexural Modulus 1.04e+6 psi
@Temperature 80.0 °C
ISO 178
 1.26e+6 psi
@Temperature 22.8 °C
ISO 178
Flexural Strain at Break 3.5 %
@Temperature 80.0 °C
at flexural strength; ISO 178
Charpy Impact Unnotched 36.0 ft-lb/in²
@Temperature -30.0 °C
ISO 179/1eU
 51.0 ft-lb/in²
@Temperature 22.8 °C
ISO 179/1eU
Charpy Impact, Notched 19.0 ft-lb/in²
@Temperature 22.8 °C
ISO 179/1eA
 20.0 ft-lb/in²
@Temperature -30.0 °C
ISO 179/1eA
 
Processing PropertiesOriginal ValueComments
Processing Temperature 158 - 176 °FHopper
 572 - 599 °FHot Runner
Feed Temperature 68.0 - 122 °FInjection
Rear Barrel Temperature 536 - 545 °F
Middle Barrel Temperature 536 - 554 °F
Front Barrel Temperature 554 - 572 °F
Nozzle Temperature 590 - 608 °F
Zone 4 572 - 590 °FInjection
Melt Temperature 590 - 608 °F
Mold Temperature 194 - 248 °F
Drying Temperature 158 - 176 °F
Dry Time 2.00 - 4.00 hour
Back Pressure <= 435 psi
Screw Speed 25 rpm
@Thickness 76.2 mm
 35 rpm
@Thickness 55.9 mm
 50 rpm
@Thickness 40.6 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHCQ6239 / 310932

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.