MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pressure Seal 201-87 Santoprene Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes:

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.960 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 86
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D2240
 86
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D2240
 86
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D2240
 86
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D2240
 86
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D2240
 86
@Temperature 150 °C,
Time 86400 sec
ASTM D2240
 87
@Temperature 150 °C,
Time 605000 sec
ASTM D2240
 87
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D2240
 87
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D2240
 87
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D2240
 87
@Temperature 125 °C,
Time 86400 sec
ASTM D2240
 87
@Temperature 125 °C,
Time 605000 sec
ASTM D2240
 87
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D2240
 87
@Temperature 100 °C,
Time 86400 sec
ASTM D2240
 87
@Temperature 100 °C,
Time 605000 sec
ASTM D2240
 87
@Time 5.00 sec
ASTM D2240
Tensile Strength 2220 psiUnaged Control; ASTM D412
 2300 psiDie C; ASTM D412
 1280 psi
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 1740 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 2150 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 2180 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 2180 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 2180 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 2210 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 2210 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 2210 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 2230 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 2260 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 2270 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 2360 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 2440 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 2460 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
Elongation at Break 540 %Unaged Control; ASTM D412
 40 %
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 240 %
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 290 %
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 430 %
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 450 %
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 490 %
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 500 %
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 520 %
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 520 %
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 530 %
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 530 %
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 530 %
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 540 %
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 540 %
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 540 %
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
Elongation, Ultimate 530 %ASTM D412
Tensile Modulus 5.40 MPa
@Temperature 125 °C
Young's modulus; ASTM D797.89
 9.20 MPa
@Temperature 100 °C
Young's modulus; ASTM D797.89
 113 MPa
@Temperature 23.0 °C
Young's modulus; ASTM D797.89
100% Modulus 1000 psiASTM D412
 1010 psiUnaged Control; ASTM D412
 1020 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 1030 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 1030 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 1030 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 1070 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 1080 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 1080 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 1090 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 1110 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 1140 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 1170 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 1180 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 1260 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 1380 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
Flexural Modulus 103 MPa0.5 in/min. Secant modulus, 1%; ASTM D 790
Tear Strength 133 pli
@Temperature 100 °C
ASTM D624
 278 pli
@Temperature 25.0 °C
ASTM D624
Compression Set 35 %
@Temperature 25.0 °C,
Time 79200 sec
ASTM D395, Method B
 52 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395, Method B
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -78.0 °FASTM D746
 
Descriptive Properties
Tension Set0.33ASTM D412

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL261 / 318471

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.