MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Addiplast Addinyl A2 ZV30 Nylon 66, 30% Glass Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Glass fiber reinforced, increased thermal aging stability

Information provided by Addiplast.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.37 g/ccISO 1183/A
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 80Conditioned; ISO 868
 85ISO 868
Tensile Strength at Break 135 MPaConditioned; ISO R 527
 180 MPaISO R 527
Elongation at Yield 3.0 %ISO R 527
 5.0 %Conditioned; ISO R 527
Modulus of Elasticity 5.80 GPaConditioned; ISO 178
 8.20 GPaISO 178
Izod Impact, Notched (ISO) 11.0 kJ/m²ISO 180/1A
 16.0 kJ/m²Conditioned; ISO 180/1A
Charpy Impact Unnotched 55.0 kJ/m²ISO 179/IeU
 65.0 kJ/m²Conditioned; ISO 179/IeU
Charpy Impact, Notched 10.0 kJ/m²ISO 179/IeA
 15.0 kJ/m²Conditioned; ISO 179/IeA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmConditioned; CEI 60093
 1.00e+15 ohm-cmCEI 60093
Dielectric Strength 30.0 kV/mmConditioned; CEI 60243-1
 35.0 kV/mmCEI 60243-1
Comparative Tracking Index 600 VCEI 60112/Solution A
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 µm/m-°CASTM E831
Melting Point 260 °CISO 3146/C2
Deflection Temperature at 1.8 MPa (264 psi) 255 °CISO 75-2/AF

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Shinkong Synthetic Fibers Shinite® N601G30 Nylon 66, 30% Glass Filled
Shinkong Synthetic Fibers Shinite® F602G30 Nylon 66, 30% Glass Filled, Fire Retardant, Halogen Free
Addiplast Addinyl A2 V30 Nylon 66, 30% Glass Filled

PFADD854 / 156068

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.