MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pressure Seal 201-80 Santoprene Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes:

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.970 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 81
@Temperature 100 °C,
Time 86400 sec
ASTM D2240
 81
@Temperature 100 °C,
Time 605000 sec
ASTM D2240
 81
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D2240
 81
@Temperature 125 °C,
Time 86400 sec
ASTM D2240
 82
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D2240
 82
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D2240
 83
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D2240
 83
@Temperature 150 °C,
Time 605000 sec
ASTM D2240
 83
@Temperature 125 °C,
Time 605000 sec
ASTM D2240
 83
@Temperature 150 °C,
Time 86400 sec
ASTM D2240
 84
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D2240
 84
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D2240
 85
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D2240
 85
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D2240
 88
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D2240
 80
@Time 5.00 sec
ASTM D2240
Tensile Strength 1400 psiUnaged Control; ASTM D412
 1600 psiDie C; ASTM D412
 1110 psi
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 1290 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 1310 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 1320 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 1380 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 1390 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 1400 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 1440 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 1440 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 1450 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 1490 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 1520 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 1530 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 1620 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 1740 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
Elongation at Break 430 %Unaged Control; ASTM D412
 130 %
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
 250 %
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 330 %
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 340 %
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 340 %
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 360 %
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 370 %
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 370 %
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 390 %
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 400 %
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 400 %
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 400 %
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 400 %
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 410 %
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 420 %
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
Elongation, Ultimate 450 %ASTM D412
Tensile Modulus 2.90 MPa
@Temperature 125 °C
Young's modulus; ASTM D797.89
 9.50 MPa
@Temperature 100 °C
Young's modulus; ASTM D797.89
 32.0 MPa
@Temperature 23.0 °C
Young's modulus; ASTM D797.89
100% Modulus 640 psiUnaged Control; ASTM D412
 700 psiASTM D412
 650 psi
@Temperature 150 °C,
Time 86400 sec
ASTM D412
 680 psi
@Temperature 125 °C,
Time 86400 sec
ASTM D412
 690 psi
@Temperature 100 °C,
Time 2.59e+6 sec
ASTM D412
 690 psi
@Temperature 100 °C,
Time 3.60e+6 sec
ASTM D412
 690 psi
@Temperature 100 °C,
Time 86400 sec
ASTM D412
 690 psi
@Temperature 100 °C,
Time 605000 sec
ASTM D412
 700 psi
@Temperature 100 °C,
Time 1.30e+6 sec
ASTM D412
 710 psi
@Temperature 125 °C,
Time 605000 sec
ASTM D412
 730 psi
@Temperature 150 °C,
Time 605000 sec
ASTM D412
 750 psi
@Temperature 125 °C,
Time 1.30e+6 sec
ASTM D412
 750 psi
@Temperature 125 °C,
Time 2.59e+6 sec
ASTM D412
 770 psi
@Temperature 125 °C,
Time 3.60e+6 sec
ASTM D412
 840 psi
@Temperature 150 °C,
Time 1.30e+6 sec
ASTM D412
 930 psi
@Temperature 150 °C,
Time 2.59e+6 sec
ASTM D412
 1000 psi
@Temperature 150 °C,
Time 3.60e+6 sec
ASTM D412
Flexural Modulus 46.0 MPa0.5 in/min. Secant modulus, 1%; ASTM D 790
Tear Strength 75.0 pli
@Temperature 100 °C
ASTM D624
 194 pli
@Temperature 25.0 °C
ASTM D624
Compression Set 27 %
@Temperature 25.0 °C,
Time 79200 sec
ASTM D395, Method B
 39 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395, Method B
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -81.0 °FASTM D746
 
Descriptive Properties
Tension Set0.2ASTM D412

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL259 / 318469

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.