MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Trivalence Technologies Polymers

(Viewing data as-entered. Click here to return)
Trivalence Technologies TriVEX™ 16FR5 HF Polycarbonate (PC) + Siloxane
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Siloxane

Material Notes: Polycarbonate, high flow, flame retardant, 5VA, impact modified, extreme cold temperature impact, weatherable, available with UV and/or release

Typical Applications: Appliance, electrical, lawn-garden, automotive, military, rescue, sporting goods

Information provided by Trivalence Technologies.

Vendors: Trivalence Technologies offers solution driven Custom Compounding, Distribution and Applied Sciences to the world’s plastic injection and extrusion markets. We pair our leading-edge resins and blends with personal attention to each customer’s needs. We work with you one-on-one at every stage and at every level to make sure you have an exceptional experience every time. Click to view more about the services we offer.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.19 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 in/in
@Thickness 3.20 mm
TVT Internal Test
Melt Flow 15 g/10 minASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 118ASTM D785
Tensile Strength at Break 9000 psiASTM D638
Elongation at Break 120 %ASTM D638
Flexural Modulus 380000 psiASTM D790
Izod Impact, Notched 10.0 ft-lb/in
@Temperature -40.0 °C
ASTM D257
 16.0 ft-lb/in
@Temperature 22.8 °C
ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 34.0 µin/in-°FASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 272 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 252 °FASTM D648
Vicat Softening Point 284 °FASTM D1525
Flammability, UL94 V-0
@Thickness 1.52 mm
TVT Internal Test
 5VA
@Thickness 3.05 mm
TVT Internal Test
 
Processing PropertiesOriginal ValueComments
Melt Temperature 550 - 600 °F
Mold Temperature 140 - 195 °F
Drying Temperature 230 - 250 °F
@Time 10800 - 21600 sec
Moisture Content 0.020 %
 
Descriptive Properties
AvailabilityEurope
 Latin America
 North America
CharacteristicHigh Flow
 Impact Modified
 Injection
 Siloxane
 Superior Impact
 UL 94 5VA TVT Internal
 UL 94V0 TVT Internal
ColorAll, Opaque
FormPellets
Outdoor Suitability (QUV)PassTVT Internal Test, "U" Grade

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTRIV9799 / 313669

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.