MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pressure Seal 23711 Ethylene Propylene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 23711 is a 70 durometer black colored high strength EPDM rubber formulated specifically for use in alkalis and acids, with the exception of concentrated sulfuric and nitric acid. It exhibits good resistance to heat and compression set. This, coupled with its good low temperature flexibility, allows for its use over a wide temperature range. Compound 23711 is also very resistant to polar materials such as water, phosphate esters, ketones and alcohols. The phosphate ester resistance makes it very useful for automotive brake fluid applications. Further, it demonstrates excellent resistance to weathering and steam. It is also a peroxide cured compound. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 AA 720 A13 C12 EA14 F17 EA14; 3 AA 720 B13 B33 C12 F17 EA14; 4 AA 720 A13 B13 B33 C12 F17 EA14; 5 AA 720 A13 B13 B33 C12 F17 EA14; 2 BA 720 C12 F17; 3 BA 720 A14 B13 C12 F17 F19; 4 BA 720 A14 C12 F17; 5 BA 720 F17 F19 C12; 6 BA 720 B13 C12; 3 CA 710 A25 B44 B35 EA14 C32 F17 F18 F19 G11 G21; 4 CA 720 A25 B35 EA14 C32 F17 F18 F19 G11 G21; 5 CA 720 A25 B35 EA14 C32 G11 G21; 2 DA 720 A26 B36 C32 EA14 F19 G11 G21; 3 DA 720 A26 C32 EA14 F19 G11 G21
Compound 23711 is UL approved per JOHX2 for water, steam, air and inert gasses. This compound is also suitable for use in anhydrous ammonia.

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.10 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 72
 64
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methyl Ethyl Ketone
 69
@Treatment Temp. 23.0 °C,
Time 252000 sec
Nitric Acid
 69
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
DOT #3 Brake Fluid
 69
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #5 Brake Fluid
 69
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
DOT #5 Brake Fluid
 69
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #4 Brake Fluid
 70
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
DOT #4 Brake Fluid
 70
@Treatment Temp. 120 °C,
Time 252000 sec
SAE Compatibility Fluid
 70
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
SAE Compatibility Fluid
 70
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #3 Brake Fluid
 70
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methanol
 71
@Treatment Temp. 100 °C,
Time 252000 sec
Sodium Hydroxide
 72
@Treatment Temp. 150 °C,
Time 252000 sec
50% Ethylene Glycol/50% H20
 72
@Treatment Temp. 150 °C,
Time 252000 sec
Ethylene Glycol
 72
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 72
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 72
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 73
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 73
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 74
@Treatment Temp. 23.0 °C,
Time 252000 sec
Hydrochloric Acid
 76
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged
 76
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 2478 psi
 842.5 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 1903.1 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methyl Ethyl Ketone
 2235.2 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Nitric Acid
 2364 psi
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #5 Brake Fluid
 2478 psi
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #4 Brake Fluid
 2552.3 psi
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 2567.2 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 2567.2 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 2579.6 psi
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 2579.6 psi
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged
 2596.9 psi
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #3 Brake Fluid
 2616.8 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methanol
 2629.2 psi
@Treatment Temp. 120 °C,
Time 252000 sec
SAE Compatibility Fluid
 2631.6 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Sodium Hydroxide
 2651.5 psi
@Treatment Temp. 150 °C,
Time 252000 sec
50% Ethylene Glycol/50% H20
 2852.2 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 2943.9 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Hydrochloric Acid
 2983.5 psi
@Treatment Temp. 150 °C,
Time 252000 sec
Ethylene Glycol
Elongation, Ultimate 351 %
 307.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methyl Ethyl Ketone
 326.1 %
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 331 %
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged
 331 %
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 332 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 334.2 %
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #4 Brake Fluid
 334.2 %
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #5 Brake Fluid
 348.9 %
@Treatment Temp. 120 °C,
Time 252000 sec
SAE Compatibility Fluid
 352.1 %
@Treatment Temp. 100 °C,
Time 252000 sec
Sodium Hydroxide
 352.1 %
@Treatment Temp. 150 °C,
Time 252000 sec
50% Ethylene Glycol/50% H20
 354.2 %
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #3 Brake Fluid
 357 %
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 360.8 %
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 370 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 371 %
@Treatment Temp. 150 °C,
Time 252000 sec
Ethylene Glycol
 375.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methanol
 380.8 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Hydrochloric Acid
 391 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Nitric Acid
100% Modulus 371 psi
Tear Strength 207 pliDie B
 210 pliDie C
Compression Set 10.2 %
@Treatment Temp. 100 °C,
Time 79200 sec
Solid
 11.2 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
Solid
 12.1 %
@Treatment Temp. 100 °C,
Time 79200 sec
Plied
 12.2 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
Plied
 13.3 %
@Treatment Temp. 125 °C,
Time 79200 sec
Solid
 15.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
Solid
 17.4 %
@Treatment Temp. 100 °C,
Time 252000 sec
Plied
 18.5 %
@Treatment Temp. 125 °C,
Time 79200 sec
Plied
 24.2 %
@Treatment Temp. 150 °C,
Time 79200 sec
Solid
 44 %
@Treatment Temp. 150 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -89.0 °F
Shrinkage -1.30 %
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
Volume, DOT #4 Brake Fluid
 -1.00 %
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
Volume, DOT #3 Brake Fluid
 -0.800 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, Ethylene Glycol
 -0.500 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, 50% Ethylene Glycol/50% H20
 -0.200 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, SAE Compatibility Fluid
 -0.200 %
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
Volume, SAE Compatibility Fluid
 0.10 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Sodium Hydroxide
 0.10 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Methanol
 0.30 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, DOT #3 Brake Fluid
 0.30 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 1.0 %
@Treatment Temp. 248 °C,
Time 1.08e+6 sec
Volume, DOT #5 Brake Fluid
 2.1 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, DOT #4 Brake Fluid
 2.1 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, DOT #5 Brake Fluid
 3.0 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Hydrochloric Acid
 8.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Nitric Acid
 11.2 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Methyl Ethyl Ketone
 
Descriptive Properties
ColorBlack
TR-10 Temperature-44.4°CASTM D1329 (10% Retraction)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL225 / 318435

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.