MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

STAR Thermoplastic Alloys & Rubbers StarGrip GP 25-9000 TPE
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: Product Description: StarGrip GP 25-9000 is an easy processing TPE designed for injection molding and this particular class of TPE material with excellent grip properties.

Features:
Soft Touch
Rubbery Feel
High Tackiness
Non-slip

Processing Method: Injection Molding

Information Provided by STAR Thermoplastic Elastomers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.900 g/cc0.900 g/ccASTM D792
Viscosity 5000 cP
@Shear Rate 10994 1/s,
Temperature 210 °C
5000 cP
@Shear Rate 10994 1/s,
Temperature 410 °F
ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 25
@Time 10.0 sec
25
@Time 0.00278 hour
ASTM D2240
Tensile Strength at Break 1.62 MPa
@Time 7200 sec
235 psi
@Time 2.00 hour
Die C; ASTM D414
Elongation at Break 735 %
@Time 7200 sec
735 %
@Time 2.00 hour
Die C; ASTM D412
300% Modulus 0.655 MPa
@Time 7200 sec,
Strain 300 %
95.0 psi
@Time 2.00 hour,
Strain 300 %
Die C; ASTM D412
Tear Strength 8.77 kN/m50.0 pliASTM D624
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kraton® D4433 P (SIS) Linear Block Copolymer
Kraton® D1112P (SIS) Linear Block Copolymer
Elastocon TPE Technologies Elastocon® 2810 Thermoplastic Elastomer
ELASTO UK Dryflex® 500300S SEBS Based Material, Unfilled Qualities, 30A Hardness, Translucent
Celanese SO.F.TER Laprene® 830.859 TPE

PSTAQ948 / 131257

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.