MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Overview of materials for Polypropylene, Mineral Reinforced
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Mineral Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene, Mineral Reinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.905 - 3.15 g/ccAverage value: 1.14 g/cc Grade Count:567
Filler Content 10.0 - 75.0 %Average value: 40.5 % Grade Count:25
Water Absorption 0.0200 - 0.0500 %Average value: 0.0289 % Grade Count:9
Moisture Absorption at Equilibrium 0.100 %Average value: 0.100 % Grade Count:3
Water Absorption at Saturation 0.100 %Average value: 0.100 % Grade Count:3
Maximum Moisture Content 0.0100Average value: 0.0100 Grade Count:19
Linear Mold Shrinkage 0.000900 - 0.0600 cm/cmAverage value: 0.00951 cm/cm Grade Count:247
Linear Mold Shrinkage, Transverse 0.00100 - 0.0200 cm/cmAverage value: 0.0110 cm/cm Grade Count:74
Melt Flow 0.500 - 100 g/10 minAverage value: 15.1 g/10 min Grade Count:544
Ash 8.00 - 70.0 %Average value: 26.5 % Grade Count:54
 6.00 - 40.0 %
@Temperature 600 - 700 °C
Average value: 22.0 % Grade Count:24
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 43.0 - 103Average value: 79.3 Grade Count:61
Hardness, Shore A 70.0 - 80.0Average value: 75.3 Grade Count:3
Hardness, Shore D 55.0 - 78.0Average value: 71.3 Grade Count:24
Ball Indentation Hardness 23.0 - 90.0 MPaAverage value: 51.1 MPa Grade Count:33
Tensile Strength, Ultimate 6.00 - 75.0 MPaAverage value: 24.7 MPa Grade Count:240
 7.00 - 16.0 MPa
@Temperature 60.0 - 120 °C
Average value: 11.4 MPa Grade Count:4
Tensile Strength, Yield 10.0 - 85.3 MPaAverage value: 26.3 MPa Grade Count:339
Elongation at Break 0.500 - 870 %Average value: 50.3 % Grade Count:249
 6.00 - 35.0 %
@Temperature 60.0 - 90.0 °C
Average value: 58.3 % Grade Count:5
Elongation at Yield 2.00 - 100 %Average value: 7.49 % Grade Count:166
 3.40 - 10.0 %
@Temperature 60.0 - 90.0 °C
Average value: 6.61 % Grade Count:5
Modulus of Elasticity 0.950 - 8.50 GPaAverage value: 2.51 GPa Grade Count:239
 0.500 - 4.90 GPa
@Temperature 60.0 - 90.0 °C
Average value: 1.37 GPa Grade Count:5
Flexural Yield Strength 14.0 - 127 MPaAverage value: 39.0 MPa Grade Count:216
Flexural Modulus 0.239 - 13.0 GPaAverage value: 2.38 GPa Grade Count:495
 0.560 - 1.25 GPa
@Temperature 60.0 - 120 °C
Average value: 0.893 GPa Grade Count:1
Izod Impact, Notched 0.200 - 100 J/cmAverage value: 0.684 J/cm Grade Count:171
 0.1471 - 10.0 J/cm
@Temperature -40.0 - 0.000 °C
Average value: 0.482 J/cm Grade Count:15
 0.196133 - 0.220 J/cm
@Temperature -30.0 - -10.0 °C
Average value: 0.482 J/cm Grade Count:10
 0.196133 - 0.220 J/cm
@Thickness 3.20 - 6.40 mm
Average value: 0.482 J/cm Grade Count:10
Izod Impact, Unnotched 1.33 J/cm - NBAverage value: 4.86 J/cm Grade Count:10
 1.0678 - 1.0678 J/cm
@Temperature -18.0 - -18.0 °C
Average value: 1.07 J/cm Grade Count:1
Izod Impact, Notched (ISO) 1.00 - 57.0 kJ/m²Average value: 13.8 kJ/m² Grade Count:147
 1.70 - 43.0 kJ/m²
@Temperature -40.0 - 10.0 °C
Average value: 5.54 kJ/m² Grade Count:46
Izod Impact, Unnotched (ISO) 17.0 kJ/m² - NBAverage value: 49.7 kJ/m² Grade Count:22
 21.0 - 200 kJ/m²
@Temperature -20.0 - -20.0 °C
Average value: 72.5 kJ/m² Grade Count:4
Charpy Impact Unnotched 0.300 J/cm² - NBAverage value: 4.30 J/cm² Grade Count:167
 0.500 J/cm² - NB
@Temperature -40.0 - 0.000 °C
Average value: 3.29 J/cm² Grade Count:98
Charpy Impact, Notched 0.150 - 7.00 J/cm²Average value: 1.38 J/cm² Grade Count:268
 0.0300 - 3.50 J/cm²
@Temperature -40.0 - 0.000 °C
Average value: 0.403 J/cm² Grade Count:164
Gardner Impact 0.678 - 22.6 JAverage value: 9.26 J Grade Count:5
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 100 - 1.00e+16 ohm-cmAverage value: 9.61e+14 ohm-cm Grade Count:28
Surface Resistance 3000 - 1.00e+16 ohmAverage value: 4.59e+14 ohm Grade Count:29
Dielectric Strength 24.0 - 43.0 kV/mmAverage value: 39.7 kV/mm Grade Count:14
Comparative Tracking Index 400 - 600 VAverage value: 576 V Grade Count:33
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 - 100 µm/m-°CAverage value: 58.3 µm/m-°C Grade Count:39
Melting Point 105 - 218 °CAverage value: 164 °C Grade Count:85
Maximum Service Temperature, Air 75.0 - 140 °CAverage value: 107 °C Grade Count:17
Deflection Temperature at 0.46 MPa (66 psi) 65.0 - 160 °CAverage value: 112 °C Grade Count:307
Deflection Temperature at 1.8 MPa (264 psi) 18.3 - 150 °CAverage value: 69.5 °C Grade Count:309
Vicat Softening Point 36.0 - 161 °CAverage value: 106 °C Grade Count:190
Brittleness Temperature -60.0 °CAverage value: -60.0 °C Grade Count:3
UL RTI, Electrical 65.0 - 120 °CAverage value: 76.0 °C Grade Count:9
UL RTI, Mechanical with Impact 65.0 - 120 °CAverage value: 76.0 °C Grade Count:9
UL RTI, Mechanical without Impact 65.0 - 120 °CAverage value: 76.0 °C Grade Count:9
Flammability, UL94 HB - 5VBGrade Count:104
Flame Spread 22.0 - 100 mm/minAverage value: 61.5 mm/min Grade Count:11
Oxygen Index 21.0 - 29.0 %Average value: 25.3 % Grade Count:15
Glow Wire Test 650 - 960 °CAverage value: 865 °C Grade Count:34
 
Optical PropertiesOriginal ValueComments
Transmission, Visible 0.100 - 92.0 %Average value: 36.0 % Grade Count:3
 
Processing PropertiesOriginal ValueComments
Processing Temperature 180 - 260 °CAverage value: 213 °C Grade Count:32
Nozzle Temperature 200 - 240 °CAverage value: 219 °C Grade Count:73
Melt Temperature 171 - 280 °CAverage value: 218 °C Grade Count:226
Mold Temperature 20.0 - 90.0 °CAverage value: 47.8 °C Grade Count:289
Injection Velocity 20.0 - 200 mm/secAverage value: 143 mm/sec Grade Count:34
Drying Temperature 60.0 - 120 °CAverage value: 80.7 °C Grade Count:152
Moisture Content 0.0100 - 0.200 %Average value: 0.116 % Grade Count:7
Injection Pressure 29.4 - 120 MPaAverage value: 80.6 MPa Grade Count:45

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene, Molded
Overview of materials for Polypropylene Copolymer
Overview of materials for Polypropylene with 40% Glass Fiber Filler
Overview of materials for Polypropylene with 40% Talc Filler
Overview of materials for Polypropylene with 20% Glass Fiber Filler

O4730 / 78388

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.