MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Raschig Group 2568 AMC
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Polyester, TS

Material Notes: Glass fiber-reinforced polyester molding compound. Very good mechanical strength, very good electrical properties and dimensional stability, heat resistant up to 500°C for short time - usable for solder baths, excellent processability with very short cycle times, low mould wear. This product meets the allowed upper limits for heavy metals and PCAs and also conforms to the requirements of the EU directives 2002/95 (RoHS), 2002/96 (WEEE) and 2006/122 (PFOS).

Processing: Injection or Transfer.

Applications: Connectors, Bobbins, Housings and Mounting plates

Information provided by the Raschig Group

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.00 - 2.20 g/ccISO 1183
Apparent Bulk Density 0.800 - 0.950 g/ccISO 60
Water Absorption <= 0.30 %
@Temperature 23.0 °C,
Time 86400 sec
ISO 62
Linear Mold Shrinkage 0.0025 - 0.0045 cm/cmInjection and Compression; ISO 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 35.0 - 60.0 MPaCompression; ISO 527
 60.0 - 70.0 MPaInjection; ISO 527
Modulus of Elasticity 6.00 - 9.00 GPaCompression; ISO 527
 13.0 - 15.0 GPaInjection; ISO 527
Flexural Strength 80.0 - 100 MPaCompression; ISO 178
 140 - 160 MPaInjection; ISO 178
Flexural Modulus 8.00 - 12.0 GPaCompression; ISO 178
 16.0 - 18.0 GPaInjection; ISO 178
Compressive Strength 120 - 170 MPaInjection; ISO 604
Charpy Impact Unnotched 0.500 - 1.00 J/cm²
@Temperature 23.0 °C
Compression; ISO 179/ 1eU
 1.50 - 1.80 J/cm²
@Temperature 23.0 °C
Injection; ISO 179/ 1eU
Charpy Impact, Notched 0.400 - 0.500 J/cm²
@Temperature 23.0 °C
Compression; ISO 179/ 1eA
 0.500 - 0.600 J/cm²
@Temperature 23.0 °C
Injection; ISO 179/ 1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 - 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+13 - 1.00e+14 ohmIEC 60093
Dielectric Constant 4.0 - 5.0
@Frequency 1e+6 Hz
IEC 60250
 5.0 - 6.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 25.0 - 35.0 kV/mmIEC 60243-1
Dissipation Factor 0.010 - 0.030
@Frequency 100 Hz
IEC 60250
 0.010 - 0.030
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.0 - 20.0 µm/m-°C
@Temperature 50.0 - 100 °C
ISO 11359-2
Thermal Conductivity 0.900 - 1.10 W/m-KASTM E1461
Deflection Temperature at 1.8 MPa (264 psi) >= 200 °CISO 75-A
Deflection Temperature at 8.0 MPa 110 - 130 °CISO 75-C
Flammability, UL94 V-0
@Thickness 1.40 mm
Shrinkage <= 0.050 %
@Temperature 110 °C,
Time 605000 sec
Post shrinkage; ISO 2577
 
Processing PropertiesOriginal ValueComments
Shelf Life 6.00 Month
@Temperature 15.0 - 25.0 °C
 
Descriptive Properties
Arc Resistance4 StufeASTM D495
Glow wire flammability test960/1IEC 60695 2-12
Glow wire ignitability test930/1IEC 60695 2-13
Water Absorption< 20 mgISO 62; 24h / 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PRASCH02 / 65287

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.