MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Tombasil, UNS C87800, Copper Casting Alloy
Categories: Metal; Nonferrous Metal; Copper Alloy; Copper Casting Alloy

Material Notes:

Casting methods recommended for this alloy: die.

Applications: Bearings, gears, impellers, rocker arms, valve stems, brush holders, bearing races, small boat propellers.

Classified under: Silicon bronzes and silicon brasses. ASTM B584; formerly ASTM B198-13B

Typical data for separately cast test bars. Alloy does not respond to heat treating. Casting shrinkage allowance is 1.9%

Key Words: Silicon Brass, ASTM B176; ASTM ZS144A
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.28 g/cc0.299 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 134134Sand cast
 163163Die cast
Hardness, Rockwell B 8585
Tensile Strength, Ultimate 460 MPa66700 psiSand cast
 585 MPa84800 psiDie cast
Tensile Strength, Yield  205 MPa
@Strain 0.5 %
29700 psi
@Strain 0.5 %
Sand cast
 310 MPa
@Strain 0.5 %
45000 psi
@Strain 0.5 %
Die cast
Elongation at Break 21 %21 %Sand cast, in 50 mm
 25 %25 %Die cast, in 50 mm
Creep Strength  9.50 MPa
@Temperature 290 °C
1380 psi
@Temperature 554 °F
for 0.00001%/h
 75.0 MPa
@Temperature 230 °C
10900 psi
@Temperature 446 °F
for 0.00001%/h
 195 MPa
@Temperature 175 °C
28300 psi
@Temperature 347 °F
for 0.00001%/h
Rupture Strength  20.0 MPa
@Temperature 290 °C,
Time 3.60e+8 sec
2900 psi
@Temperature 554 °F,
Time 100000 hour
 125 MPa
@Temperature 230 °C,
Time 3.60e+8 sec
18100 psi
@Temperature 446 °F,
Time 100000 hour
Modulus of Elasticity 106 GPa15400 ksiSand cast
 138 GPa20000 ksiDie cast
Compressive Strength 183 MPa26500 psiat permanent set of 0.1%
 515 MPa74700 psiat permanent set of 10%
Fatigue Strength  150 MPa
@# of Cycles 1.00e+8
21800 psi
@# of Cycles 1.00e+8
rotating beam
 150 MPa
@# of Cycles 5.00e+7 - 2.00e+8
21800 psi
@# of Cycles 5.00e+7 - 2.00e+8
 170 MPa
@# of Cycles 6.00e+6 - 5.00e+7
24700 psi
@# of Cycles 6.00e+6 - 5.00e+7
 205 MPa
@# of Cycles 600000 - 4.00e+6
29700 psi
@# of Cycles 600000 - 4.00e+6
 240 MPa
@# of Cycles 100000 - 600000
34800 psi
@# of Cycles 100000 - 600000
 275 MPa
@# of Cycles 60000 - 250000
39900 psi
@# of Cycles 60000 - 250000
Machinability 40 %40 %UNS C36000 (free-cutting brass) = 100%
Charpy Impact 43.0 J31.7 ft-lbV-notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000284 ohm-cm
@Temperature 20.0 °C
0.0000284 ohm-cm
@Temperature 68.0 °F
 0.0000284 ohm-cm
@Temperature 15.0 °C
0.0000284 ohm-cm
@Temperature 59.0 °F
 0.0000287 ohm-cm
@Temperature 35.0 °C
0.0000287 ohm-cm
@Temperature 95.0 °F
 0.0000291 ohm-cm
@Temperature 60.0 °C
0.0000291 ohm-cm
@Temperature 140 °F
 0.0000294 ohm-cm
@Temperature 85.0 °C
0.0000294 ohm-cm
@Temperature 185 °F
 0.0000297 ohm-cm
@Temperature 120 °C
0.0000297 ohm-cm
@Temperature 248 °F
 0.0000302 ohm-cm
@Temperature 150 °C
0.0000302 ohm-cm
@Temperature 302 °F
 0.0000305 ohm-cm
@Temperature 175 °C
0.0000305 ohm-cm
@Temperature 347 °F
 0.0000310 ohm-cm
@Temperature 205 °C
0.0000310 ohm-cm
@Temperature 401 °F
 0.0000315 ohm-cm
@Temperature 230 °C
0.0000315 ohm-cm
@Temperature 446 °F
 0.0000318 ohm-cm
@Temperature 255 °C
0.0000318 ohm-cm
@Temperature 491 °F
 0.0000323 ohm-cm
@Temperature 285 °C
0.0000323 ohm-cm
@Temperature 545 °F
Magnetic Permeability 1.01.0
 
Thermal PropertiesMetricEnglishComments
CTE, linear  17.1 µm/m-°C
@Temperature 75.0 °C
9.50 µin/in-°F
@Temperature 167 °F
 17.5 µm/m-°C
@Temperature 105 °C
9.72 µin/in-°F
@Temperature 221 °F
 17.8 µm/m-°C
@Temperature 130 °C
9.89 µin/in-°F
@Temperature 266 °F
 18.3 µm/m-°C
@Temperature 160 °C
10.2 µin/in-°F
@Temperature 320 °F
 18.7 µm/m-°C
@Temperature 185 °C
10.4 µin/in-°F
@Temperature 365 °F
 18.9 µm/m-°C
@Temperature 210 °C
10.5 µin/in-°F
@Temperature 410 °F
 19.1 µm/m-°C
@Temperature 240 °C
10.6 µin/in-°F
@Temperature 464 °F
 19.5 µm/m-°C
@Temperature 270 °C
10.8 µin/in-°F
@Temperature 518 °F
 19.6 µm/m-°C
@Temperature 20.0 - 260 °C
10.9 µin/in-°F
@Temperature 68.0 - 500 °F
 19.7 µm/m-°C
@Temperature 295 °C
10.9 µin/in-°F
@Temperature 563 °F
 19.9 µm/m-°C
@Temperature 325 °C
11.1 µin/in-°F
@Temperature 617 °F
Specific Heat Capacity 0.375 J/g-°C0.0896 BTU/lb-°F
Thermal Conductivity  26.0 W/m-K
@Temperature 20.0 °C
180 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 27.0 W/m-K
@Temperature 35.0 °C
187 BTU-in/hr-ft²-°F
@Temperature 95.0 °F
 28.0 W/m-K
@Temperature 20.0 °C
194 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 29.0 W/m-K
@Temperature 70.0 °C
201 BTU-in/hr-ft²-°F
@Temperature 158 °F
 32.0 W/m-K
@Temperature 95.0 °C
222 BTU-in/hr-ft²-°F
@Temperature 203 °F
 34.0 W/m-K
@Temperature 120 °C
236 BTU-in/hr-ft²-°F
@Temperature 248 °F
 36.0 W/m-K
@Temperature 150 °C
250 BTU-in/hr-ft²-°F
@Temperature 302 °F
 38.0 W/m-K
@Temperature 175 °C
264 BTU-in/hr-ft²-°F
@Temperature 347 °F
 39.0 W/m-K
@Temperature 200 °C
271 BTU-in/hr-ft²-°F
@Temperature 392 °F
 42.0 W/m-K
@Temperature 230 °C
291 BTU-in/hr-ft²-°F
@Temperature 446 °F
 44.0 W/m-K
@Temperature 260 °C
305 BTU-in/hr-ft²-°F
@Temperature 500 °F
 46.0 W/m-K
@Temperature 290 °C
319 BTU-in/hr-ft²-°F
@Temperature 554 °F
Melting Point 821 - 917 °C1510 - 1680 °F
Solidus 821 °C1510 °F
Liquidus 917 °C1680 °F
Shrinkage 1.5 - 1.9 %1.5 - 1.9 %Patternmaker's Shrinkage
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 260 °C500 °FStress-Relieving Temperature
Casting Temperature 955 - 980 °C1750 - 1800 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.15 %<= 0.15 %
Copper, Cu 80 - 83 %80 - 83 %
Iron, Fe <= 0.15 %<= 0.15 %
Lead, Pb <= 0.15 %<= 0.15 %
Magnesium, Mg <= 0.010 %<= 0.010 %
Manganese, Mn <= 0.15 %<= 0.15 %
Other, total <= 0.25 %<= 0.25 %
Silicon, Si 3.75 - 4.25 %3.75 - 4.25 %
Tin, Sn <= 0.25 %<= 0.25 %
Zinc, Zn 14 %14 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tombasil, UNS C87500, Copper Casting Alloy
Silicon Yellow Brass, UNS C87900, Copper Casting Alloy
Leaded Yellow Brass, UNS C85800, Copper Casting Alloy, Die Castings
Leaded Semi-Red Brass (Valve Metal), UNS C84400, Copper Casting Alloy
Leaded Semi-Red Brass, UNS C84800, Copper Casting Alloy

MC87800b1 / 11924

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.