MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Carpenter Custom 450® Stainless Steel, Condition H1000 (Age Hardened 538°C (1000°F))
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Data provided by Carpenter Technology Corporation.

Custom 450® stainless is a martensitic age-hardenable stainless steel which exhibits very good corrosion resistance (similar to that of Stainless Type 304) with moderate strength (similar to that of Stainless Type 410). the alloy has a yield strength somewhat greater than 100 ksi (689 MPa) in the annealed condition, but is easily fabricated. A single-step aging treatment develops higher strength with good ductility and toughness. This stainless can be machined, hot-worked, and cold-formed in the same manner as other martensitic age-hardenable stainless steels. A particular advantage is ease of welding and brazing. Custom 450 stainless is generally supplied in the annealed condition, requiring no heat treatment by the user for many applications. Because it has corrosion resistance like Type 304 stainless but three times the yield strength, it has been used in applications where Type 304 was not strong enough. On the other hand, it has also replaced Type 410 stainless directly on a strength basis where Type 410 had insufficient corrosion resistance. Mechanical properties will depend on the aging temperature selected.

Custom 450® is a registered trademark of Carpenter Technology Corporation.

Key Words: UNS S45000
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.76 g/cc0.280 lb/in³H900 Condition
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 360360Estimated from Rockwell C for 3000 kg load, 10 mm ball Brinell measurement.
Hardness, Knoop 392392Estimated from Rockwell C
Hardness, Rockwell C 3939
Hardness, Vickers 376376Estimated from Rockwell C
Tensile Strength, Ultimate 1193 MPa173000 psi
Tensile Strength, Yield 1165 MPa
@Strain 0.2 %
169000 psi
@Strain 0.2 %
Elongation at Break 17 %17 %In 4D
Reduction of Area 63 %63 %
Modulus of Elasticity 200 GPa29000 ksi
Notched Tensile Strength 1882 MPa273000 psiKt = 10
Poissons Ratio 0.290.29
Fatigue Strength 94.0 MPa
@# of Cycles 1.00e+7
13600 psi
@# of Cycles 1.00e+7
R.R. Moore Test, Smooth Rotating Beam
Shear Modulus 77.5 GPa11200 ksiCalculated
Charpy Impact 69.0 J50.9 ft-lbV-notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000846 ohm-cm0.0000846 ohm-cmH900 Condition
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.8 µm/m-°C
@Temperature 24.0 - 93.0 °C
6.00 µin/in-°F
@Temperature 75.2 - 199 °F
H900 Condition
 10.87 µm/m-°C
@Temperature 24.0 - 260 °C
6.039 µin/in-°F
@Temperature 75.2 - 500 °F
H900 Condition
 11.75 µm/m-°C
@Temperature 24.0 - 593 °C
6.528 µin/in-°F
@Temperature 75.2 - 1100 °F
H900 Condition
Specific Heat Capacity 0.477 J/g-°C0.114 BTU/lb-°F
Thermal Conductivity  15.0 W/m-K
@Temperature 23.0 °C
104 BTU-in/hr-ft²-°F
@Temperature 73.4 °F
condition H 900
 18.2 W/m-K
@Temperature 200 °C
126 BTU-in/hr-ft²-°F
@Temperature 392 °F
condition H 900
 24.4 W/m-K
@Temperature 500 °C
169 BTU-in/hr-ft²-°F
@Temperature 932 °F
condition H 900
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.050 %<= 0.050 %min. Nb content = 8 x C content
Chromium, Cr 14 - 16 %14 - 16 %
Copper, Cu 1.25 - 1.75 %1.25 - 1.75 %
Iron, Fe 75 %75 %as remainder
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 0.50 - 1.0 %0.50 - 1.0 %
Nickel, Ni 5.0 - 7.0 %5.0 - 7.0 %
Phosphorus, P <= 0.030 %<= 0.030 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition H1050
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 1025
Carpenter Custom 450® Stainless Steel, Annealed
Carpenter Custom 450® Stainless Steel, Condition H900 (Age Hardened 482°C)
Carpenter Custom 450® Stainless Steel, Condition H1150 (Age Hardened 621°C)

NCAR8F / 15670

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.