MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
RTP Company RTP 3405-4 Liquid Crystal Polymer (LCP), Glass Fiber - UL94 V-0
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled

Material Notes: The RTP 3400 series of compounds is based on a self-reinforcing crystalline polyer. Liquid crystal polymers offer outstanding heat and chemical resistance. These unique properties combined with excellent processability lend these compounds to a diverse range of applications.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.61 g/ccASTM D 792
Filler Content 30 %Primary Additive
Linear Mold Shrinkage 0.00020 - 0.0010 cm/cm
@Thickness 3.17 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 105ASTM D 785
Tensile Strength at Break 17000 psiASTM D 638
Elongation at Break 1.0 - 2.0 %ASTM D 638
Tensile Modulus 2300 ksiASTM D 638
Flexural Strength 24000 psiASTM D 790
Flexural Modulus 2100 ksiASTM D 790
Izod Impact, Notched 1.80 ft-lb/in
@Thickness 3.17 mm
D 256
Izod Impact, Unnotched 10.0 ft-lb/in
@Thickness 3.17 mm
ASTM D4812
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.1
@Frequency 1e+6 Hz
Dry; ASTM D 150
Dielectric Strength 650 V/milShort Term; in oil; ASTM D 149
Dissipation Factor 0.030
@Frequency 1e+6 Hz
Dry; ASTM D 150
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 580 °FASTM D 648
Flammability, UL94 V-0
@Thickness 0.300 mm
 V-0
@Thickness 1.59 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 685 - 750 °F
Mold Temperature 150 - 200 °F
Drying Temperature 300 °F
Dry Time 8 hour
Dew Point -20.0 °F
Injection Pressure 10000 - 18000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Stanyl® TE250F6 PA46-GF30 FR(17), Dry, 30% Glass Filled, Heat Stabilized, Flame Retardant
RTP Company RTP 3405-3 Liquid Crystal Polymer (LCP), Glass Fiber
Celanese Vectra® C130 Liquid Crystal Polymer (LCP), 30% Glass Reinforced
RTP Company ESD 3482-1 Liquid Crystal Polymer (LCP); Carbon Fiber - Electrically Conductive - (Preliminary Data Sheet)
Avient Edgetek® LCP-30CF/000 Liquid Crystal Polymer - 30% Carbon Fiber

PQZWA1262 / 90709

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.