MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Techmer ES HiFill® ABS IM TM20 20% Mineral Filled
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Impact Grade, Molded; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Availability: North America

Forms: Pellets

Filler/Reinforcement: Mineral Filler, 20% Filler by Weight

Additive: Impact Modifier

Features: Impact Modified

Processing Method: Injection Molding

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.19 g/ccASTM D792
Water Absorption 0.13 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0015 in/in
@Thickness 3.17 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 107ASTM D785
Tensile Strength 10600 psiASTM D638
Elongation at Yield 3.5 %ASTM D638
Flexural Yield Strength 15800 psiASTM D790
Flexural Modulus 570000 psiASTM D790
Izod Impact, Notched 1.90 ft-lb/in
@Thickness 3.17 mm
ASTM D256
Izod Impact, Unnotched 9.50 ft-lb/in
@Thickness 3.17 mm
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmASTM D257
Dielectric Strength 450 V/milMethod A (Short-Time); ASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 19.0 µin/in-°FASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 233 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 218 °FUnannealed; ASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), PTFE Filled
LG Chemical XG570 MABS, Anti-Scratch, High Impact, High Flow
LG Chemical LUMID HI5083A(W) PA6/ABS+MF8%, High Impact
LATI Latishield 36/AR-10A-V0E ABS, Steel Fiber Reinforced, Flame Retardant
Elix Polymers ELIX™ 190 TE Acrylonitrile Butadiene Styrene (ABS), PTFE Reinforced

PTPC0035 / 135973

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.