MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
RTP Company RTP 2099 X 121241 B Bio-Based Polylactic Acid (PLA); PC-PLA Blend - ESD Protection - Permanently Anti-static - 26% Renewable Resource Content
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polylactic Acid (PLA) Biopolymer

Material Notes: For detailed processing information, see the PLA Molding Guide on the RTP Company website.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D 792
Linear Mold Shrinkage 0.0060 cm/cm
@Thickness 3.20 mm
ASTM D 955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 5200 psiASTM D 638
Elongation at Break 7.0 %ASTM D 638
Tensile Modulus 250 ksiASTM D 638
Flexural Strength 8000 psiASTM D 790
Flexural Modulus 250 ksiASTM D 790
Izod Impact, Notched 1.00 ft-lb/in
@Thickness 3.20 mm
ASTM D 256
Izod Impact, Unnotched 16.0 ft-lb/in
@Thickness 3.20 mm
ASTM D 4812
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+8 - 1.00e+11 ohm-cmASTM D 257
Surface Resistivity per Square 1.00e+10 - 1.00e+12 ohmASTM D 257
Static Decay <= 2.0 secMIL-PRF-81705D, 5kV to 50 V, 12% RH; FTMS101C; 4046.1
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 185 °FASTM D 648
Flammability, UL94 HB
@Thickness 1.50 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 430 - 470 °F
Mold Temperature 75.0 - 160 °F
Drying Temperature 175 °F
@Time 14400 sec
Moisture Content 0.020 %
Dew Point -40.0 °F
Injection Pressure 8000 - 15000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eastman Tenite 285A2R30020 Cellulose Acetate Butyrate, Natural, Trsp
FKuR Kunststoff Terralene® LL 1303 Biobased Polyethylene
Rotuba MSS Cellulose Acetate
Celanese Riteflex® 655A TPC, Unfilled
Arkema Pebax® Rnew® 40R53 SP 01 Polyether Block Amide (PEBA)

PQZUA15386 / 134667

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.