MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

BASF Ultramid® T KR 4357 G6 Nylon 6/6T, 30% Glass Fiber Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes: Product Description: Ultramid® T KR 4357 G6 is a 30% glass fiber reinforced, impact-modified, injection-molding PA6/6T grade. High toughness, stiffness and strength, low water absorption. High melting point (295°C). After the material has been conditioned, its mechanical properties remain stable up to 60°C.

Availability: Asia Pacific; Europe; North America

Filler/Reinforcement: Glass Fiber, 30% Filler by Weight

Additive: Impact Modifier

Features: Copolymer; Good Toughness; High Stiffness; High Strength; Impact Modified; Low to No Water Absorption

Agency Ratings: EC 1907/2006 (REACH)

RoSH Compliance: RoSH Compliant

Automotive Specifications: GM QK 001303 Type A Color: 564 Black

Forms: Pellets

Processing Method: Injection Molding

Information provided by BASF Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.37 g/cc0.0495 lb/in³ISO 1183
Water Absorption 0.80 %0.80 %Equilibrium, 50% RH; ISO 62
Water Absorption at Saturation 4.5 %4.5 %ISO 62
Maximum Moisture Content 0.150.15
 
Mechanical PropertiesMetricEnglishComments
Tensile Stress  165 MPa
@Temperature 22.8 °C
23900 psi
@Temperature 73.0 °F
ISO 527-2
 249 MPa
@Temperature -40.0 °C
36100 psi
@Temperature -40.0 °F
ISO 527-2
Elongation at Break  3.5 %
@Temperature 22.8 °C
3.5 %
@Temperature 73.0 °F
ISO 527-2
 3.6 %
@Temperature -40.0 °C
3.6 %
@Temperature -40.0 °F
ISO 527-2
Tensile Modulus 9.31 GPa1350 ksiISO 527-1
Izod Impact, Notched (ISO) 23.1 kJ/m²11.0 ft-lb/in²ISO 180
Charpy Impact Unnotched  9.03 J/cm²
@Temperature -30.0 °C
43.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 9.45 J/cm²
@Temperature 22.8 °C
45.0 ft-lb/in²
@Temperature 73.0 °F
ISO 179
Charpy Impact, Notched  1.01 J/cm²
@Temperature -30.0 °C
4.80 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 1.89 J/cm²
@Temperature 22.8 °C
9.00 ft-lb/in²
@Temperature 73.0 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Dielectric Constant 4.3
@Frequency 1e+6 Hz
4.3
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.030
@Frequency 1e+6 Hz
0.030
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 25.2 µm/m-°C14.0 µin/in-°F
CTE, linear, Transverse to Flow 55.8 µm/m-°C31.0 µin/in-°F
Melting Point 295 °C563 °FISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 240 °C464 °FUnannealed; ISO 75-2/A
UL RTI, Electrical  140 °C
@Thickness 0.762 mm
284 °F
@Thickness 0.0300 in
UL 746B
 140 °C
@Thickness 1.52 mm
284 °F
@Thickness 0.0600 in
UL 746B
 140 °C
@Thickness 3.05 mm
284 °F
@Thickness 0.120 in
UL 746B
UL RTI, Mechanical with Impact  100 °C
@Thickness 0.762 mm
212 °F
@Thickness 0.0300 in
UL 746B
 110 °C
@Thickness 1.52 mm
230 °F
@Thickness 0.0600 in
UL 746B
 115 °C
@Thickness 3.05 mm
239 °F
@Thickness 0.120 in
UL 746B
UL RTI, Mechanical without Impact  120 °C
@Thickness 0.762 mm
248 °F
@Thickness 0.0300 in
UL 746B
 140 °C
@Thickness 1.52 mm
284 °F
@Thickness 0.0600 in
UL 746B
 140 °C
@Thickness 3.05 mm
284 °F
@Thickness 0.120 in
UL 746B
 
Processing PropertiesMetricEnglishComments
Melt Temperature 310 - 330 °C590 - 626 °F
Mold Temperature 80.0 - 120 °C176 - 248 °F
Drying Temperature 110 °C230 °F
Dry Time <= 8.00 hour<= 8.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASG2036 / 310729

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.