MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

(Viewing data as-entered. Click here to return)
Magnesium Elektron Elektron® ZK60A Magnesium Alloy, UNS M16600
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: ZK60A is a wrought magnesium base alloy containing zinc and zirconium. Increased strength is obtained by artificial aging from the as-fabricated form. ZK60A-T5 has the best combination of strength and ductility at room-temperature of the wrought magnesium alloys.

Applications: Forgings in ZK60A find application in high strength parts for use primarily where the service temperature is below 150°C. ZK60A forgings can be used where pressure tightness or machinability are required. That parts are dimensionally stable during and after machining is also an important design consideration. Forgings in ZK60A find application in high strength parts for satellites, helicopter gearboxes and rotor hubs, bicycle frames, road wheels, missile frames and interstage fairings, brake housings and landing gear struts.

Information provided by Magnesium Elektron.

Key Words: UNS M16600; AMS4362; ASTM B91; FEDERAL QQ-M-40
Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.83 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell E 77ZK60A-T5
 85ZK60A-T6
Tensile Strength at Break >= 290 MPaMin Design Specification per ZK60A-T5, Die Forgings
 >= 295 MPaMin Design Specification per ZK60A-T6, Die Forgings
 100 MPa
@Temperature 200 °C
 205 MPa
@Temperature 100 °C
 310 MPa
@Temperature 20.0 °C
Tensile Strength, Yield >= 180 MPa
@Strain 0.2 %
Min Design Specification per ZK60A-T5, Die Forgings
 >= 220 MPa
@Strain 0.2 %
Min Design Specification per ZK60A-T6, Die Forgings
 75.0 MPa
@Strain 0.2 %,
Temperature 200 °C
 150 MPa
@Strain 0.2 %,
Temperature 100 °C
 200 MPa
@Strain 0.2 %,
Temperature 20.0 °C
Elongation at Break >= 3.0 %Min Design Specification per ZK60A-T6, Die Forgings
 >= 6.0 %Min Design Specification per ZK60A-T5, Die Forgings
 13 %
@Temperature 22.0 °C
in 5.65 A½
 30 %
@Temperature 100 °C
 50 %
@Temperature 200 °C
Creep Strength 5.00 MPa
@Temperature 150 °C,
Time 360000 sec
0.2% creep
 7.00 MPa
@Temperature 150 °C,
Time 36000 sec
0.2% creep
 12.0 MPa
@Temperature 150 °C,
Time 360000 sec
0.5% creep
 16.0 MPa
@Temperature 150 °C,
Time 36000 sec
0.5% creep
 20.0 MPa
@Temperature 100 °C,
Time 360000 sec
0.2% creep
 20.0 MPa
@Temperature 150 °C,
Time 3600 sec
0.2% creep
 35.0 MPa
@Temperature 150 °C,
Time 3600 sec
0.5% creep
 37.0 MPa
@Temperature 100 °C,
Time 36000 sec
0.2% creep
 45.0 MPa
@Temperature 100 °C,
Time 360000 sec
0.5% creep
 60.0 MPa
@Temperature 100 °C,
Time 360000 sec
1% creep
 70.0 MPa
@Temperature 100 °C,
Time 36000 sec
0.5% creep
 90.0 MPa
@Temperature 100 °C,
Time 36000 sec
1% creep
Modulus of Elasticity 45.0 GPa
Compressive Yield Strength 160 MPa
@Strain 0.2 %
Ultimate Bearing Strength 420 MPa
Bearing Yield Strength 285 MPa
@Strain 0.2 %
Poissons Ratio 0.35
Fatigue Strength 122 MPa
@# of Cycles 1.00e+7
Rotating bend
 128 MPa
@# of Cycles 1.00e+6
Rotating bend
 160 MPa
@# of Cycles 100000
Rotating bend
Fracture Toughness 34.0 MPa-m½KIC
Shear Strength 165 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000570 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 27.1 µm/m-°C
Specific Heat Capacity 1.10 J/g-°C
Thermal Conductivity 121 W/m-K
Melting Point 520 - 635 °C
Solidus 520 °C
Liquidus 635 °C
Maximum Service Temperature, Air 150 °C
 
Component Elements PropertiesOriginal ValueComments
Magnesium, Mg 93.8 - 94.75 %As Balance
Zinc, Zn 4.8 - 6.2 %
Zirconium, Zr >= 0.45 %
 
Descriptive Properties
Corrosion rate50 mpyASTM B117 Salt spray test

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
SAE SiC/AZ91 Magnesium Matrix Composite, as cast
Magnesium EA55RS-T4, Extruded
Magnesium EA65RS-T4, Extruded
SAE AZ91 Magnesium Matrix Composite, as cast
Magnesium Elektron Elektron® WE54 Magnesium Casting Alloy, UNS M18410

NMAGEL909 / 186924

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.