MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ Copolymer DMX9455A Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LEXAN DMX9455A is a standard flow, flame retardant and transparent polycarbonate copolymer resin with improved scratch resistance and improved dielectric performance (lower Df). It is a good candidate for applications such as 5G related devices and anti-scratch covers.

Features: Easy Flow,Transparent

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.176 g/ccASTM D792
 1.20 g/ccASTM D792
Density 1.17 g/ccASTM D792
 1.17 g/ccISO 1183
Water Absorption 0.080 %
@Time 86400 sec
ASTM D570
Moisture Absorption 0.0200 %Injection Molding
 0.0400 %23°C/50% RH/24 hrs; ASTM D570
 0.130 %23°C / 50% RH; ISO 62
Moisture Absorption at Equilibrium 0.13 %23°C/50% RH; ASTM D570
Water Absorption at Saturation 0.27 %ISO 62-1
 0.28 %ASTM D570
Viscosity 13 cP
@Load 1.20 kg,
Temperature 300 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 14.5 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell L 108ASTM D785
Hardness, Rockwell M 93ASTM D785
Ball Indentation Hardness 128 MPaH358/30; ISO 2039-1
Tensile Strength at Break 60.0 MPa50 mm/min; ISO 527
 65.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 80.0 MPa50 mm/min; ASTM D638
 80.0 MPa50 mm/min; ISO 527
Elongation at Break 40 %50 mm/min; ISO 527
 70 %50 mm/min; ASTM D638
Elongation at Yield 7.0 %50 mm/min; ASTM D638
 7.0 %50 mm/min; ISO 527
Tensile Modulus 2450 MPa1 mm/min; ISO 527
 2900 MPa50 mm/min; ASTM D638
Flexural Strength 108 MPayield, 2 mm/min; ISO 178
 120 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2450 MPa2 mm/min; ISO 178
 2600 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 30.0 JASTM D256
 30.0 J
@Temperature -30.0 °C
ASTM D256
Izod Impact, Unnotched NBASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*3; ISO 180/1A
 4.00 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NB80*10*3; ISO 180/1U
 45.0 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1U
Charpy Impact Unnotched NBEdgew 80*10*3 sp=62mm; ISO 179/1eU
 47.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 3.00 kJ/m²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 3.00 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 30.0 JASTM D3763
Taber Abrasion, mg/1000 Cycles 10CS-17, 1 kg; ASTM D1044
 10CS-17, 1 kg; SABIC method
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 175 - 250 VUL 746A
Hot Wire Ignition, HWI 15 - 30 sec
@Thickness >=1.00 mm
UL 746A
 30 - 60 sec
@Thickness >=3.00 mm
UL 746A
High Amp Arc Ignition, HAI >= 120 arcs
@Thickness >=1.00 mm
UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature -40.0 - 95.0 °C
ASTM E831
 70.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature -40.0 - 95.0 °C
ASTM E831
 70.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
Specific Heat Capacity 1.40 J/g-°CASTM C351
Thermal Conductivity 0.200 W/m-KASTM C177
 0.200 W/m-KISO 8302
Hot Ball Pressure Test 125 °CPASS; IEC 60695-10-2
 140 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 131 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 133 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 118 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 119 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 138 °CRate B/50; ISO 306
 139 °CRate B/50; ASTM D1525
 140 °CRate B/120; ISO 306
UL RTI, Electrical 80.0 °CUL 746B
UL RTI, Mechanical with Impact 80.0 °CUL 746B
UL RTI, Mechanical without Impact 80.0 °CUL 746B
Flammability, UL94 HB
@Thickness >=0.400 mm
UL 94
 V-2
@Thickness >=1.50 mm
UL 94
 V-0
@Thickness >=2.50 mm
UL 94
Glow Wire Ignition Temperature 825 °C
@Thickness 3.00 mm
IEC 60695-2-13
 850 °C
@Thickness 1.00 mm
IEC 60695-2-13
 850 °C
@Thickness 2.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 1.00 mm
IEC 60695-2-12
 960 °C
@Thickness 2.00 mm
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.584ASTM D542
 1.584ISO 489
Haze <= 0.80 %
@Thickness 2.54 mm
ASTM D1003
Transmission, Visible 88 %
@Thickness 2.54 mm
ASTM D1003
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °CInjection Molding
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
Precipitation Temperature 60.0 - 80.0 °CHopper Temperature
 
Descriptive Properties
Erichson scratch depth, 6N14 micrometerSABIC method
Pencil Hardness test, 1kgfHASTM D3363

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80127 / 288074

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.