MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

(Viewing data as-entered. Click here to return)
Magnesium Elektron Elektron® AZ91E Magnesium Casting Alloy
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: ELEKTRON AZ91E is a general purpose gravity sand casting alloy containing aluminum, zinc and manganese. Good properties may be achieved particularly with the use of chills in the mold. Corrosion resistance is excellent.

Applications: The alloy may be used in aerospace casting applications particularly where there is no high temperature requirement or a requirement for pressure tightness.

Information provided by Magnesium Elektron.

Key Words: ASTM B80 AZ91E; BS2970 MAG7/3; DIN MgAl /19 Zn1; AFNOR G-A9Z1; BS2L125; ISO 16220 MC21120
Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.81 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 75
Tensile Strength at Break >= 117 MPaMin Design Specification per ASTM B80 AZ91E; T6 condition
 260 MPaTypical, T4
 270 MPaTypical, T6
Tensile Strength, Yield >= 83.0 MPa
@Strain 0.2 %
Min Design Specification per ASTM B80 AZ91E; T6 condition
 125 MPa
@Strain 0.2 %
Typical, T4
 170 MPa
@Strain 0.2 %
Typical, T6
Elongation at Break >= 2.0 %Min Design Specification per ASTM B80 AZ91E; T6 condition
 4.5 %Typical, T6
 9.0 %Typical, T4
Modulus of Elasticity 44.0 GPa
Compressive Yield Strength 130 MPa
@Strain 0.2 %
Compressive Strength 400 MPa
Poissons Ratio 0.35
Fatigue Strength 70.0 MPa
@# of Cycles 5.00e+7
Rotating Bend
Fracture Toughness 13.2 MPa-m½KIC
Shear Strength 140 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000141 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 27.0 µm/m-°C
Specific Heat Capacity 1.00 J/g-°C
Thermal Conductivity 84.0 W/m-K
Melting Point 470 - 595 °C
Solidus 470 °C
Liquidus 595 °C
Shrinkage 1.3 %Pattern Makers Shrinkage Factor
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 8.1 - 9.3 %
Magnesium, Mg 89.35 - 91.33 %As Balance
Manganese, Mn 0.17 - 0.35 %
Zinc, Zn 0.40 - 1.0 %
 
Descriptive Properties
Corrosion rate<50 mpyASTM B117 Salt spray test
Damping Index0.2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium Elektron Elektron® AZ31B Magnesium Extrusion Alloy, UNS M11311
Magnesium Elektron Elektron® ZRE1 Magnesium Alloy, UNS M12330
Magnesium Elektron Elektron® 43 Magnesium Extrusion Alloy, UNS M18434
Magnesium Elektron Elektron® W28 Magnesium Alloy Welding Rod Composition
Magnesium Elektron Elektron® W7 Magnesium Alloy Welding Rod Composition

NMAGEL901 / 186916

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.