MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Plastcom SLOVASTER® B BT Polyethylene Terephthalate  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Features

PBT basic type for injection moulding. Melt is characterized by outstanding fluidity, which enables injection moulding of complicated and divided products also on multiple moulds. Anisotropy of shrinkage enables injection moulding of round, cylindrical or other hole products. Delivered in natural and in the full RAL color scale.

Application: Injection Moulding

Information Provided by Plastcom spol. s r.o.

Key Words: PBT
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.31 g/cc0.0473 lb/in³STN 64 0111
Linear Mold Shrinkage 0.018 cm/cm0.018 in/inSTN 64 0808
Linear Mold Shrinkage, Transverse 0.0193 cm/cm0.0193 in/inSTN 64 0808
Melt Flow 40 g/10 min
@Load 2.16 kg,
Temperature 230 °C
40 g/10 min
@Load 4.76 lb,
Temperature 446 °F
STN EN ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 55.0 MPa7980 psiSTN EN ISO 527-2
Elongation at Break 8.0 %8.0 %STN EN ISO 527-2
Tensile Modulus 2.50 GPa363 ksiSTN EN ISO 527-2
Flexural Strength 80.0 MPa11600 psiSTN EN ISO 178
Flexural Modulus 2.50 GPa363 ksiSTN EN ISO 178
Charpy Impact Unnotched  13.0 J/cm²
@Temperature 23.0 °C
61.9 ft-lb/in²
@Temperature 73.4 °F
STN EN ISO 179
 13.0 J/cm²
@Temperature -20.0 °C
61.9 ft-lb/in²
@Temperature -4.00 °F
STN EN ISO 179
Charpy Impact, Notched 0.160 J/cm²
@Temperature 23.0 °C
0.761 ft-lb/in²
@Temperature 73.4 °F
STN EN ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm1.00e+17 ohm-cmSTN IEC 60093
Surface Resistance 1.00e+15 ohm1.00e+15 ohmSTN IEC 60093
Dielectric Strength 23.0 kV/mm584 kV/inSTN IEC 60243
Comparative Tracking Index 600 V600 VSTN 34 6468
 
Thermal PropertiesMetricEnglishComments
Melting Point 200 - 220 °C392 - 428 °FDSC; STN EN ISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C131 °FSTN EN ISO 75/A
Vicat Softening Point 200 °C392 °FB; STN EN ISO 306
Flammability, UL94 HBHB
Glow Wire Test 850 °C1560 °FSTN IEC 60695-2-10
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 270 °C482 - 518 °F
Mold Temperature 50.0 - 80.0 °C122 - 176 °F
Drying Temperature 120 °C248 °F
Dry Time 4 hour4 hour
Moisture Content 0.050 %0.050 %STN EN ISO 960
Injection Pressure 60.0 - 100 MPa8700 - 14500 psi

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aclo Accucomp Polycarbonate POL051L Medium Viscosity
Avient Gravi-Tech™ GRV-PS-027-BA-WHT Polybutylene Terephthalate (PBT)
Barlog Plastics KEBATER B510 PBT unreinforced
Celanese Celanex® 1400A PBT, Unfilled
Evonik Vestodur® 2000 Medium Viscosity PBT

PPLACO099 / 106977

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.