MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Plastcom SLOVALEN PC 88 FRD 1 Polypropylene Copolymer, Halogen Flame Retardant, UV Stabilized
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer; Polypropylene, Flame Retardant

Material Notes: Features

Modified copolymer PP with the possibility of changing the MFI within the interval 5 - 20 g/10min. Stabilized against the UV-radiation by the UV stabilizer on the HALS basis. Retarded with the halogen flame retardant. Application - stadium seats with guaranteed life-cycle of the mechanical and surface properties, electrical industry - terminals, coil forms, covers of electrotools, guides. Fulfills 960°C glow wire and flammability in accordance with UL 94 V2. Concerning flammability, it complies with the building norm DIN 4102-B2. Delivered in the full RAL color scale.

Application: Injection Moulding

Information Provided by Plastcom spol. s r.o.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.930 g/ccSTN 64 0111
Linear Mold Shrinkage 0.0244 cm/cmSTN 64 0808
Linear Mold Shrinkage, Transverse 0.0239 cm/cmSTN 64 0808
Melt Flow 12 g/10 min
@Load 2.16 kg,
Temperature 230 °C
STN EN ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 28.0 MPaSTN EN ISO 527-2
Elongation at Break 20 %STN EN ISO 527-2
Tensile Modulus 1200 MPaSTN EN ISO 527-2
Flexural Strength 35.0 MPaSTN EN ISO 178
Flexural Modulus 1000 MPaSTN EN ISO 178
Charpy Impact Unnotched 110 kJ/m²
@Temperature -20.0 °C
STN EN ISO 179
 NB
@Temperature 23.0 °C
STN EN ISO 179
Charpy Impact, Notched 4.00 kJ/m²
@Temperature -20.0 °C
STN EN ISO 179
 9.00 kJ/m²
@Temperature 23.0 °C
STN EN ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmSTN IEC 60093
Surface Resistance 1.00e+16 ohmSTN IEC 60093
Dielectric Strength 24.0 kV/mmSTN IEC 60243
Comparative Tracking Index 450 VSTN 34 6468
 
Thermal PropertiesOriginal ValueComments
Melting Point 150 °CDSC; STN EN ISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °CSTN EN ISO 75/A
Vicat Softening Point 110 °CB; STN EN ISO 306
Flammability, UL94 V-2
Glow Wire Test 960 °CSTN IEC 60695-2-10
 
Processing PropertiesOriginal ValueComments
Melt Temperature 200 - 250 °C
Mold Temperature 30.0 - 50.0 °C
Injection Pressure 50.0 - 80.0 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Plastcom SLOVALEN PC 78 FRD 1 Polypropylene Copolymer, Halogen Flame Retardant, UV Stabilized
Overview of materials for Polypropylene Copolymer
Cossa Polimeri ESTAPROP K 0200 V2 Flame Retardant Polypropylene
Cossa Polimeri ESTAPROP 1006 V2 K Flame Retardant Polypropylene
Cossa Polimeri ESTAPROP 1006 V2 H Flame Retardant Polypropylene

PPLACO094 / 106972

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.