MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow Isoplast® 151 Polyurethane (PUR-RT), Impact Modified  (discontinued **)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: ISOPLAST® 151 resin is an impact modified amorphous polymer with the chemical resistance of crystalline resins. Its outstanding properties include excellent chemical resistance, high heat, low moisture sensitivity, toughness, and dimensional stability.

Data provided by Dow Chemical.

Key Words: TPUR
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccASTM Data
Water Absorption 0.17 %
Linear Mold Shrinkage 0.0050 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 120
Tensile Strength, Ultimate 48.3 MPaASTM Data
Tensile Strength, Yield 57.9 MPaASTM Data
Elongation at Break 120 %ASTM Data
Elongation at Yield 6.5 %ISO Data
Tensile Modulus 1.59 GPaASTM Data
Izod Impact, Notched 5.87 J/cmASTM Data
Charpy Impact Unnotched NBISO Data
 NBISO Data, Low Temp
Charpy Impact, Notched 1.20 J/cm²ISO Data, Low Temp
 6.70 J/cm²ISO Data
Instrumented Impact Total Energy 67.8 J
@Temperature -30.0 °C
 67.8 J
@Temperature 23.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 77.0 µm/m-°C
@Temperature 20.0 °C
ISO data
Deflection Temperature at 0.46 MPa (66 psi) 98.9 °CUnannealed; ASTM Data
 110 °CAnnealed; ASTM Data
Deflection Temperature at 1.8 MPa (264 psi) 85.6 °CUnannealed; 104°C (219°F) annealed; ASTM Data
Vicat Softening Point 117 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
A. Schulman DuraGrip™ DGR 6030 NC/BK Thermoplastic Elastomer (TPE)
3M Scotch-Weld™ EZ250150 Polyurethane Reactive (PUR) Easy 250 Wood Adhesive
Covestro Baydur® GS PUR Polyurethane
Dow Isoplast® 202 Polyurethane (PUR-RT), Impact Modified
Isoflon PUR Polyurethane

PDW060 / 34291

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.