MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AlphaGary Evoprene™ COGEE 638 SEBS Thermoplastic Elastomer  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Styrenic TPE

Material Notes: Evoprene™ COGEE was developed to comold or coextrude with engineered thermoplastics and designed for soft touch applications.
Processing: compatible with polypropylene and polystyrene for co-molding or co-extrusion

Alphagary is part of Orbia.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.990 g/ccISO 2781
Viscosity Measurement 9.0
@Temperature 150 °C
Kg/cm2; Macklow-Smith extrusion rheometer
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 65ISO 868
Tensile Strength 5.80 MPaISO 37
Elongation at Break 398 %ISO 37
100% Modulus 0.00250 GPa
@Strain 100 %
ISO 37
300% Modulus 0.00430 GPa
@Strain 300 %
ISO 37
Adhesive Bond Strength 1.77 MPa
Tear Strength 48.0 kN/mISO 34-B
Abrasion 165mm3; DIN 53516
Compression Set 50 %
@Temperature 23.0 °C,
Time 259000 sec
ISO 815
 87 %
@Temperature 100 °C,
Time 79200 sec
ISO 815
 88 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 60.0 °C
Minimum Service Temperature, Air -30.0 °C
 
Descriptive Properties
Ozone ResistanceNo Cracks100 pphm / 200 hrs / 20% strain, ISO1431

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AlphaGary Evoprene™ COGEE 631 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ COGEE 637 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ G 6087 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ G 614 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ G 940 SEBS Thermoplastic Elastomer

PGARY9749 / 140542

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.