MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Entec Hylex® P2010L Polycarbonate  (discontinued **)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: Entec's proprietary products include a full range of compounds in the Nylon 6/6, Nylon 6, ABS, PBT, Polycarbonate, PC/ABS, PC/ASA, PC/PBT, and PPO/PPE resin families.

Information provided by Entec.

This grade is no longer in production

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccASTM D792
Water Absorption 0.15 %24 hrs; ASTM D570
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cmASTM D955
Melt Flow 10 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 80ASTM D785
Tensile Strength at Break 8800 psiASTM D638
Elongation at Break 110 %ASTM D638
Flexural Strength 12100 psiASTM D790
Flexural Modulus 330000 psiASTM D790
Izod Impact, Notched 14.0 ft-lb/in73°F, 0.125 in; ASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 265 °FUnannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 520 - 540 °F
Middle Barrel Temperature 530 - 550 °F
Front Barrel Temperature 540 - 570 °F
Nozzle Temperature 530 - 570 °F
Melt Temperature 550 - 600 °F
Mold Temperature 170 - 200 °F
Drying Temperature 250 °F
Dry Time 3 - 12 hour
Moisture Content <= 0.020 %
Injection Pressure 1000 - 1800 psi
Back Pressure 70.0 - 150 psi
Shot Size 40 - 60 %
Screw Speed 40 - 70 rpm
 
Descriptive Properties
Holding Pressure700 to 1200 psi

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Polymer Resources PC/ABS-GP1 General Purpose PC/ABS Alloy
Entec Hylex® P2007L Polycarbonate
Covestro Makrolon® 2407 Polycarbonate, Injection Grade

PENT068 / 36105

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.