MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Hifax CA 387 A Thermoplastic Polyolefin
Categories: Polymer; Thermoplastic; Polyolefin

Material Notes: Hifax polypropylene resins based on the Catalloy process are used in applications such as building and construction (e.g., single-ply roofing), industrial applications (e.g., wire and cable), and automotive industries. Hifax priovides good processability, excellent impact resistance, a broad range of stiffness from very soft to rigid products, high temperature resistance and low linear coefficient of thermal expansion.

Hifax CA 387 A is a reactor TPO (thermoplastic polyolefin) manufactured using LyondellBasell's proprietary Catalloy process technology. It has high melt flow and an excellent balance of impact, stiffness, processability and paintability. Hifax CA 387 A is primarily used for painted automotive bumper fascias that require high durability, and for other injection molded parts with paintable and weatherable requirements. It is also utilized as a component in compounded materials for a wide range of industrial applications. The grade is available in natural pellet form. Applications: Bumpers, Caps & Closures, Exterior Automotive Applications, Interior Automotive Applications, Polymer Modifier.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.890 g/cc0.0322 lb/in³method A; ISO 1183-1
Melt Flow 18.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
18.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 52
@Time 15.0 sec
52
@Time 0.00417 hour
ISO 868
Tensile Strength at Break 13.0 MPa1890 psiISO 527-1,-2
Tensile Strength, Yield 18.0 MPa2610 psiISO 527-1,-2
Elongation at Break 110 %110 %ISO 527-1,-2
Elongation at Yield 8.0 %8.0 %ISO 527-1,-2
Flexural Modulus 1.00 GPa145 ksiISO 178
Charpy Impact, Notched  0.260 J/cm²
@Temperature -40.0 °C
1.24 ft-lb/in²
@Temperature -40.0 °F
failure mode- complete break; ISO 179
 0.870 J/cm²
@Temperature -20.0 °C
4.14 ft-lb/in²
@Temperature -4.00 °F
failure mode- complete break; ISO 179
 6.00 J/cm²
@Temperature 23.0 °C
28.6 ft-lb/in²
@Temperature 73.4 °F
failure mode-partial break; ISO 179
Impact Test  17.0 J
@Temperature 23.0 °C
12.5 ft-lb
@Temperature 73.4 °F
Multi-axial Impact Strength, 2.2m/s,3.2mm plaque, failure mode: ductile; ASTM D 3763
 27.0 J
@Temperature -40.0 °C
19.9 ft-lb
@Temperature -40.0 °F
Multi-axial Impact Strength, 2.2m/s,3.2mm plaque, failure mode: ductile; ASTM D 3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 80.0 °C176 °Funannealed; ISO 75B-1,-2
Vicat Softening Point 120 °C248 °FA50; ISO 306
DSC Induction Temperature 163 °C325 °FISO 11357-3
 
Optical PropertiesMetricEnglishComments
Gloss 77 %
@Thickness 1.14 mm
77 %
@Thickness 0.0450 in
60°; ASTM D2457
 
Descriptive Properties
Processing MethodCompounding, Injection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEQT7188 / 218825

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.