MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Pressure Seal 8703 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 8703 is a 70 durometer black colored Viton® GLT. It exhibits good low temperature flexibility coupled with good heat, fluid and compression set resistance.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 720 A1-10 B37 B38 EF31 F15; 4 HK 720 A1-11 B38 EF31 EO78 F17; 6 HK 720 A1-10 A1-11 B31 B38 EF31 EO88 F15
AMS-R-83485 Type I
This Compound is RoHS Compliant

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.84 g/cc1.84 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7070
 62
@Treatment Temp. 23.0 °C,
Time 605000 sec
62
@Treatment Temp. 73.4 °F,
Time 168 hour
15% EtOH/85% FUEL C
 63
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
63
@Treatment Temp. 73.4 °F,
Time 1600 hour
15% EtOH/85% FUEL C
 64
@Treatment Temp. 200 °C,
Time 252000 sec
64
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 64
@Treatment Temp. 23.0 °C,
Time 252000 sec
64
@Treatment Temp. 73.4 °F,
Time 70.0 hour
15% EtOH/85% FUEL C
 64
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
64
@Treatment Temp. 73.4 °F,
Time 600 hour
15% EtOH/85% FUEL C
 65
@Treatment Temp. 200 °C,
Time 252000 sec
65
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 65
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
65
@Treatment Temp. 73.4 °F,
Time 600 hour
85% EtOH/15% FUEL C
 65
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
65
@Treatment Temp. 73.4 °F,
Time 1600 hour
85% EtOH/15% FUEL C
 66
@Treatment Temp. 23.0 °C,
Time 605000 sec
66
@Treatment Temp. 73.4 °F,
Time 168 hour
85% EtOH/15% FUEL C
 67
@Treatment Temp. 23.0 °C,
Time 605000 sec
67
@Treatment Temp. 73.4 °F,
Time 168 hour
Ethanol
 67
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
67
@Treatment Temp. 73.4 °F,
Time 1600 hour
Ethanol
 67
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
67
@Treatment Temp. 73.4 °F,
Time 600 hour
Ethanol
 67
@Treatment Temp. 23.0 °C,
Time 252000 sec
67
@Treatment Temp. 73.4 °F,
Time 70.0 hour
85% EtOH/15% FUEL C
 68
@Treatment Temp. 23.0 °C,
Time 252000 sec
68
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Ethanol
 69
@Treatment Temp. 23.0 °C,
Time 252000 sec
69
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 70
@Treatment Temp. 250 °C,
Time 252000 sec
70
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
 70
@Treatment Temp. 150 °C,
Time 252000 sec
70
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3 (IRM 903)
 71
@Treatment Temp. 275 °C,
Time 252000 sec
71
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 71
@Treatment Temp. 150 °C,
Time 252000 sec
71
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1 (IRM 901)
 72
@Treatment Temp. 23.0 °C,
Time 252000 sec
72
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
Tensile Strength 16.82 MPa2439 psi
 12.14 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
1761 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 13.218 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
1917.1 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 14.143 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
2051.2 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 15.892 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
2304.9 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3 (IRM 903)
 16.463 MPa
@Treatment Temp. 275 °C,
Time 252000 sec
2387.8 psi
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 16.614 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
2409.7 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 16.766 MPa
@Treatment Temp. 250 °C,
Time 252000 sec
2431.7 psi
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
 16.82 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
2439 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1 (IRM 901)
Elongation, Ultimate 273 %273 %
 209.7 %
@Treatment Temp. 200 °C,
Time 252000 sec
209.7 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 233.4 %
@Treatment Temp. 200 °C,
Time 252000 sec
233.4 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 234 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
234 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 249 %
@Treatment Temp. 150 °C,
Time 252000 sec
249 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1 (IRM 901)
 264.8 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
264.8 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 270.5 %
@Treatment Temp. 150 °C,
Time 252000 sec
270.5 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3 (IRM 903)
 313.7 %
@Treatment Temp. 275 °C,
Time 252000 sec
313.7 %
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 458.6 %
@Treatment Temp. 250 °C,
Time 252000 sec
458.6 %
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
100% Modulus 3.97 MPa576 psi
Tear Strength 22.1 kN/m126 pliDie C
 24.0 kN/m137 pliDie B
Compression Set  10 %
@Treatment Temp. 175 °C,
Time 79200 sec
10 %
@Treatment Temp. 347 °F,
Time 22.0 hour
Plied
 10.2 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
10.2 %
@Treatment Temp. 73.4 °F,
Time 22.0 hour
Plied
 11.8 %
@Treatment Temp. 200 °C,
Time 79200 sec
11.8 %
@Treatment Temp. 392 °F,
Time 22.0 hour
Plied
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -44.4 °C-48.0 °F
Shrinkage  0.40 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
0.40 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel A
 0.40 %
@Treatment Temp. 150 °C,
Time 252000 sec
0.40 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 1.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
1.7 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #3
 3.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
3.9 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, Ethanol
 5.0 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
5.0 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel C
 6.2 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
6.2 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, 85% EtOH/15% FUEL C
 6.2 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
6.2 %
@Treatment Temp. 73.4 °F,
Time 168 hour
Volume, Ethanol
 9.5 %
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
9.5 %
@Treatment Temp. 73.4 °F,
Time 1600 hour
Volume, Ethanol
 9.5 %
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
9.5 %
@Treatment Temp. 73.4 °F,
Time 600 hour
Volume, Ethanol
 9.9 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
9.9 %
@Treatment Temp. 73.4 °F,
Time 168 hour
Volume, 85% EtOH/15% FUEL C
 9.9 %
@Treatment Temp. 200 °C,
Time 252000 sec
9.9 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Volume, Service Fluid 100
 12.8 %
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
12.8 %
@Treatment Temp. 73.4 °F,
Time 1600 hour
Volume, 85% EtOH/15% FUEL C
 13 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
13 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, 15% EtOH/85% FUEL C
 13.3 %
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
13.3 %
@Treatment Temp. 73.4 °F,
Time 600 hour
Volume, 85% EtOH/15% FUEL C
 15.8 %
@Treatment Temp. 200 °C,
Time 252000 sec
15.8 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Volume, Stauffer Blend 7700
 18.7 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
18.7 %
@Treatment Temp. 73.4 °F,
Time 168 hour
Volume, 15% EtOH/85% FUEL C
 19.2 %
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
19.2 %
@Treatment Temp. 73.4 °F,
Time 1600 hour
Volume, 15% EtOH/85% FUEL C
 19.3 %
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
19.3 %
@Treatment Temp. 73.4 °F,
Time 600 hour
Volume, 15% EtOH/85% FUEL C
 
Descriptive Properties
ColorBlack
TR-10 Temperature-34°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL100 / 318310

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.