MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LATI Later 4 G/30-V0CT2 PBT, 30% Glass Fiber Reinforced, Flame Retardant
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

Material Notes: Polybutylene Terephthalate (PBT) based compound. Glass fibers. UL94 V-0 classified, with brominated flame retardants, PBB/PBDE free.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Information provided by Lati Industria Termoplastici S.p.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.65 g/cc0.0596 lb/in³
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cm0.0030 - 0.0050 in/in
Linear Mold Shrinkage, Transverse 0.0090 - 0.012 cm/cm0.0090 - 0.012 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  15.0 MPa
@Temperature 150 °C
2180 psi
@Temperature 302 °F
 20.0 MPa
@Temperature 120 °C
2900 psi
@Temperature 248 °F
 30.0 MPa
@Temperature 90.0 °C
4350 psi
@Temperature 194 °F
 55.0 MPa
@Temperature 60.0 °C
7980 psi
@Temperature 140 °F
 85.0 MPa
@Temperature 23.0 °C
12300 psi
@Temperature 73.4 °F
Elongation at Break  2.3 %
@Temperature 23.0 °C
2.3 %
@Temperature 73.4 °F
 2.6 %
@Temperature 60.0 °C
2.6 %
@Temperature 140 °F
 2.6 %
@Temperature 90.0 °C
2.6 %
@Temperature 194 °F
 2.7 %
@Temperature 120 °C
2.7 %
@Temperature 248 °F
 2.8 %
@Temperature 150 °C
2.8 %
@Temperature 302 °F
Tensile Modulus  1.80 GPa
@Temperature 150 °C
261 ksi
@Temperature 302 °F
 2.50 GPa
@Temperature 120 °C
363 ksi
@Temperature 248 °F
 3.40 GPa
@Temperature 90.0 °C
493 ksi
@Temperature 194 °F
 5.40 GPa
@Temperature 60.0 °C
783 ksi
@Temperature 140 °F
 7.80 GPa
@Temperature 23.0 °C
1130 ksi
@Temperature 73.4 °F
Charpy Impact Unnotched  3.00 J/cm²
@Temperature 23.0 °C
14.3 ft-lb/in²
@Temperature 73.4 °F
 3.50 J/cm²
@Temperature -20.0 °C
16.7 ft-lb/in²
@Temperature -4.00 °F
Charpy Impact, Notched  0.650 J/cm²
@Temperature -20.0 °C
3.09 ft-lb/in²
@Temperature -4.00 °F
 0.850 J/cm²
@Temperature 23.0 °C
4.04 ft-lb/in²
@Temperature 73.4 °F
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 400 V400 VA solution
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 135 °C275 °F
Deflection Temperature at 0.46 MPa (66 psi) 215 °C419 °F
Deflection Temperature at 1.8 MPa (264 psi) 185 °C365 °F
Vicat Softening Point 170 °C
@Load 5.00 kg
338 °F
@Load 11.0 lb
Flammability, UL94  V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
 V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
Oxygen Index 28 %28 %
Glow Wire Test  960 °C
@Thickness 1.00 mm
1760 °F
@Thickness 0.0394 in
GWFI/GWT
 960 °C
@Thickness 2.00 mm
1760 °F
@Thickness 0.0787 in
GWFI/GWT
Glow Wire Ignition Temperature  750 °C
@Thickness 1.00 mm
1380 °F
@Thickness 0.0394 in
 750 °C
@Thickness 2.00 mm
1380 °F
@Thickness 0.0787 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 230 - 250 °C446 - 482 °F
Mold Temperature 70.0 - 90.0 °C158 - 194 °F
Drying Temperature 110 - 130 °C
@Time 10800 sec
230 - 266 °F
@Time 3.00 hour
 
Descriptive Properties
ISO Shrinkage - Pressure60 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LATI LATER 4 G/20-V0 20% Glass Fiber Reinforced Polybutylene terephthalate (PBT) (UL94 V-0)
LATI Later 4 G/30-V0 PBT, 30% Glass Fiber Reinforced, Flame Retardant
LATI Later 4 G/30-V0HF1 PBT, 30% Glass Fiber Reinforced, Flame Retardant
Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled
LATI Latilub 75/4-05T G/30-V0 PBT, 30% Glass Fiber Reinforced, PTFE Filled, Flame Retardant

PLATH9780 / 177476

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.