MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Techmer ES HiFill® PVDF CF15-M BK 15% Milled Carbon Filled
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF); Polyvinylidinefluoride (PVDF), with Carbon Fiber

Material Notes: Availability: North America

Forms: Pellets

Filler/Reinforcement: Milled Carbon Fiber, 15% Filler by Weight

Appearance: Black

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.77 g/ccASTM D792
Water Absorption 0.020 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0050 in/in
@Thickness 3.17 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 106ASTM D785
Tensile Strength, Yield 13500 psiASTM D638
Elongation at Break 4.5 %ASTM D638
Flexural Yield Strength 17000 psiASTM D790
Flexural Modulus 1.24e+6 psiASTM D790
Izod Impact, Notched 1.60 ft-lb/in
@Thickness 3.17 mm
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+6 ohm-cmASTM D257
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 25.0 µin/in-°FASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 335 °FUnannealed; ASTM D648
Flammability, UL94 V-0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Techmer ES HiFill® PVDF CF15 BK 15% Carbon Filled
LNP Thermocomp® FP-VC-1003 BK8-019 Polyvinylidene Fluoride, Carbon Fiber Reinforcement
DuPont Mobility and Materials Kalrez® 1050LF FFKM Perfluoroelastomer
Arkema Kynar® 720 Polyvinylidene Fluoride Homopolymer- Injection Molding and Extrusion
Polyram RamLloy PI300G6 PVDF, 30% Glass Fiber

PTPC0598 / 136536

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.