MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Borealis GB311U Polypropylene Compound, Glass Fiber Reinforced  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 30% Glass Fiber Filler

Material Notes: GB311U is a 30% chemically coupled glass fiber reinforced polypropylene compound intended for injection molding. This material shows excellent mechanical properties also at elevated temperatures. Applications: GB311U has been developed especially for demanding applications in the automotive industry including technical components exposed to high heat and loads, washing machine parts, and structural parts.

Information provided by Borealis AG

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.12 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0020 cm/cmaverage process; 150x80x2mm
Linear Mold Shrinkage, Transverse 0.010 cm/cmaverage process; 150x80x2mm
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 124 MPa132 N/10s; ISO 2039
Tensile Strength, Yield 97.0 MPaISO 527-2
Elongation at Break 3.0 %50mm/min; ISO 527-2
Elongation at Yield 2.8 %ISO 527-2
Tensile Modulus 6800 MPa1mm/min; ISO 527-2
Flexural Strength 130 MPaISO 178
Flexural Modulus 6200 MPa2mm/min; ISO 178
Izod Impact, Notched (ISO) 8.00 kJ/m²
@Temperature -20.0 °C
ISO 180/1A
 11.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Charpy Impact Unnotched 45.0 kJ/m²ISO 179/1eU
 50.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 8.00 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 9.00 kJ/m²
@Temperature -20.0 °C
ISO 179/1eA
 11.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 159 °CISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 145 °CISO 75-2
Vicat Softening Point 135 °C
@Load 5.10 kg
ISO 306
 165 °C
@Load 1.02 kg
ISO 306
 
Processing PropertiesOriginal ValueComments
Feed Temperature 40.0 - 80.0 °C
Melt Temperature 230 - 280 °Cmass temperature
Mold Temperature 30.0 - 50.0 °C
Injection Velocity 100 - 200 mm/sec
Hold Pressure 30.0 - 60.0 MPa
 
Descriptive Properties
Back Pressureas low as possible
Emission (µgC/g)15VDA 277
Fogging (mg)0.97100°C;3h;DIN 75201
 1100°C;16h;DIN 75201
Screw Speedlow to medium

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Borealis Fibremod™ GB364WG Polypropylene Compound, Glass Fiber Reinforced
Borealis Nepol™ GB601HP Polypropylene, 30% Long Glass Fiber Reinforced w/HK060AE
A. Schulman Diamond NPP30-2000 GF30 30% Glass Filled Homopolymer Polypropylene
A. Schulman POLYFORT™ FPP 3459 Glass Filled Impact Copolymer
Adell ER-16 Homopolymer Polypropylene, 30% Glass Reinforced

PBOREA458 / 108717

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.