Physical Properties | Original Value | Comments |
---|
Specific Gravity | 1.23 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Shore A | 75 |
| 60 @Treatment Temp. 23.0 °C, Time 252000 sec |
| 64 @Treatment Temp. 23.0 °C, Time 252000 sec |
| 70 @Treatment Temp. 150 °C, Time 252000 sec |
| 72 @Treatment Temp. 100 °C, Time 252000 sec |
| 72 @Treatment Temp. 125 °C, Time 252000 sec |
| 73 @Treatment Temp. 100 °C, Time 252000 sec |
| 74 @Treatment Temp. 23.0 °C, Time 252000 sec |
| 75 @Treatment Temp. 100 °C, Time 252000 sec |
| 75 @Treatment Temp. 125 °C, Time 252000 sec |
| 75 @Treatment Temp. 150 °C, Time 252000 sec |
| 77 @Treatment Temp. 100 °C, Time 252000 sec |
| 77 @Treatment Temp. 100 °C, Time 252000 sec |
| 80 @Treatment Temp. 125 °C, Time 252000 sec |
| 80 @Treatment Temp. 125 °C, Time 252000 sec |
| 81 @Treatment Temp. 150 °C, Time 252000 sec |
Tensile Strength | 3382 psi |
| 1254.7 psi @Treatment Temp. 23.0 °C, Time 252000 sec |
| 1782.3 psi @Treatment Temp. 23.0 °C, Time 252000 sec |
| 2380.9 psi @Treatment Temp. 150 °C, Time 252000 sec |
| 3104.7 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 3128.3 psi @Treatment Temp. 23.0 °C, Time 252000 sec |
| 3297.4 psi @Treatment Temp. 100 °C, Time 252000 sec |
| 3304.2 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 3304.2 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 3365.09 psi @Treatment Temp. 150 °C, Time 252000 sec |
| 3578.2 psi @Treatment Temp. 100 °C, Time 252000 sec |
| 3578.2 psi @Treatment Temp. 100 °C, Time 252000 sec |
| 3608.6 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 3669.5 psi @Treatment Temp. 100 °C, Time 252000 sec |
| 3713.4 psi @Treatment Temp. 150 °C, Time 252000 sec |
Elongation, Ultimate | 539 % |
| 233.9 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 246.9 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 299.1 % @Treatment Temp. 150 °C, Time 252000 sec |
| 314.8 % @Treatment Temp. 125 °C, Time 252000 sec |
| 352 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 362.2 % @Treatment Temp. 100 °C, Time 252000 sec |
| 383.8 % @Treatment Temp. 125 °C, Time 252000 sec |
| 390.2 % @Treatment Temp. 100 °C, Time 252000 sec |
| 396.2 % @Treatment Temp. 150 °C, Time 252000 sec |
| 523.9 % @Treatment Temp. 125 °C, Time 252000 sec |
| 523.9 % @Treatment Temp. 125 °C, Time 252000 sec |
| 561.1 % @Treatment Temp. 150 °C, Time 252000 sec |
| 574 % @Treatment Temp. 100 °C, Time 252000 sec |
| 574.03 % @Treatment Temp. 100 °C, Time 252000 sec |
100% Modulus | 528 psi |
Tear Strength | 208 pli |
| 257 pli |
Compression Set | 10 % @Treatment Temp. 125 °C, Time 79200 sec |
| 10.9 % @Treatment Temp. 100 °C, Time 79200 sec |
| 12.4 % @Treatment Temp. 125 °C, Time 79200 sec |
| 13.2 % @Treatment Temp. 100 °C, Time 252000 sec |
| 13.4 % @Treatment Temp. 150 °C, Time 79200 sec |
| 14.5 % @Treatment Temp. 100 °C, Time 252000 sec |
| 15.1 % @Treatment Temp. 100 °C, Time 79200 sec |
| 17.4 % @Treatment Temp. 150 °C, Time 79200 sec |
|
Thermal Properties | Original Value | Comments |
---|
Brittleness Temperature | -80.0 °F |
Shrinkage | -2.60 % @Treatment Temp. 150 °C, Time 252000 sec |
| -2.50 % @Treatment Temp. 125 °C, Time 252000 sec |
| -2.00 % @Treatment Temp. 100 °C, Time 252000 sec |
| 0.80 % @Treatment Temp. 100 °C, Time 252000 sec |
| 3.0 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 8.6 % @Treatment Temp. 100 °C, Time 252000 sec |
| 12 % @Treatment Temp. 150 °C, Time 252000 sec |
| 12.8 % @Treatment Temp. 125 °C, Time 252000 sec |
| 34.5 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 56.3 % @Treatment Temp. 23.0 °C, Time 252000 sec |
|
Descriptive Properties |
---|
Color | Black |