MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
20Cr-20Ni-20Co-4W-4Mo-4(Nb+Ta) IRON BASED SUPERALLOY BARS FOR GAS TURBINE BLADES
Categories: Metal; Ferrous Metal; Tool Steel; Air-Hardening Steel

Material Notes:

Creep and rupture data provided by NIMS

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Rupture Strength 49.0 - 66.0 MPa
@Temperature 775 °C,
Time 3.60e+8 sec
 66.0 - 81.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
 82.0 - 98.0 MPa
@Temperature 725 °C,
Time 3.60e+8 sec
 101 - 116 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
 124 - 138 MPa
@Temperature 675 °C,
Time 3.60e+8 sec
 152 - 164 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
 
Component Elements PropertiesOriginal ValueComments
Chromium, Cr 18 - 22 %
Cobalt, Co 18 - 22 %
Iron, Fe 19 - 37 %As Balance
Molybdenum, Mo 3.0 - 5.0 %
Nb + Ta 3.0 - 5.0 %
Nickel, Ni 18 - 22 %
Tungsten, W 3.0 - 5.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1020 Steel, mock carburized at 915°C (1680°F) for 8 hours, 775°C (1430°F) reheat, water quenched, 175°C (350°F) temper, 13 mm (0.5 in.) round
IN-738 Cast Nickel Superalloy
MetalTek IN® 713 UNS N07713 Centri-Vac Nickel Cobalt Based Alloy
13Cr-4.5Mo-0.75Ti-6Al-2.3(Nb+Ta)-Zr-B NICKEL BASED SUPERALLOY CASTINGS FOR GAS TURBINE BLADES
19Cr-18Co-4Mo-3Ti-3Al-B NICKEL BASED SUPERALLOY CASTINGS AND FORGINGS FOR GAS TURBINE BLADES

NIMS031 / 77548

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.