Physical Properties | Original Value | Comments |
---|
Specific Gravity | 1.20 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Shore A | 73 |
| 58 @Treatment Temp. 23.0 °C, Time 252000 sec |
| 60 @Treatment Temp. 23.0 °C, Time 252000 sec |
| 67 @Treatment Temp. 150 °C, Time 252000 sec |
| 68 @Treatment Temp. 125 °C, Time 252000 sec |
| 73 @Treatment Temp. 23.0 °C, Time 252000 sec |
| 73 @Treatment Temp. 100 °C, Time 252000 sec |
| 74 @Treatment Temp. 125 °C, Time 252000 sec |
| 76 @Treatment Temp. 150 °C, Time 252000 sec |
| 78 @Treatment Temp. 125 °C, Time 252000 sec |
| 78 @Treatment Temp. 125 °C, Time 252000 sec |
| 83 @Treatment Temp. 150 °C, Time 252000 sec |
| 83 @Treatment Temp. 150 °C, Time 252000 sec |
| 87 @Treatment Temp. 175 °C, Time 252000 sec |
Tensile Strength | 2912 psi |
| 1537.5 psi @Treatment Temp. 23.0 °C, Time 252000 sec |
| 1820 psi @Treatment Temp. 23.0 °C, Time 252000 sec |
| 2746.1 psi @Treatment Temp. 175 °C, Time 252000 sec |
| 2836.3 psi @Treatment Temp. 23.0 °C, Time 252000 sec |
| 2868.3 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 2952.8 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 2952.8 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 3043 psi @Treatment Temp. 150 °C, Time 252000 sec |
| 3063.4 psi @Treatment Temp. 100 °C, Time 252000 sec |
| 3127.5 psi @Treatment Temp. 150 °C, Time 252000 sec |
| 3139.1 psi @Treatment Temp. 125 °C, Time 252000 sec |
| 3147.9 psi @Treatment Temp. 150 °C, Time 252000 sec |
| 3147.9 psi @Treatment Temp. 150 °C, Time 252000 sec |
Elongation, Ultimate | 321 % |
| 123.9 % @Treatment Temp. 175 °C, Time 252000 sec |
| 165 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 194.8 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 197.9 % @Treatment Temp. 125 °C, Time 252000 sec |
| 223.1 % @Treatment Temp. 150 °C, Time 252000 sec |
| 223.1 % @Treatment Temp. 150 °C, Time 252000 sec |
| 287.9 % @Treatment Temp. 125 °C, Time 252000 sec |
| 296 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 303.02 % @Treatment Temp. 150 °C, Time 252000 sec |
| 306.9 % @Treatment Temp. 125 °C, Time 252000 sec |
| 312.98 % @Treatment Temp. 100 °C, Time 252000 sec |
| 335.1 % @Treatment Temp. 150 °C, Time 252000 sec |
| 338.01 % @Treatment Temp. 125 °C, Time 252000 sec |
100% Modulus | 674 psi |
Tear Strength | 163 pli |
Compression Set | 5.0 % @Treatment Temp. 100 °C, Time 79200 sec |
| 6.2 % @Treatment Temp. 100 °C, Time 79200 sec |
| 7.9 % @Treatment Temp. 100 °C, Time 252000 sec |
| 12.2 % @Treatment Temp. 125 °C, Time 252000 sec |
| 20.5 % @Treatment Temp. 150 °C, Time 252000 sec |
| 31.5 % @Treatment Temp. 175 °C, Time 252000 sec |
|
Thermal Properties | Original Value | Comments |
---|
Brittleness Temperature | -82.0 °F |
Shrinkage | -4.60 % @Treatment Temp. 125 °C, Time 252000 sec |
| -4.50 % @Treatment Temp. 150 °C, Time 252000 sec |
| 1.3 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 11.1 % @Treatment Temp. 125 °C, Time 252000 sec |
| 12.4 % @Treatment Temp. 150 °C, Time 252000 sec |
| 30 % @Treatment Temp. 23.0 °C, Time 252000 sec |
| 51.5 % @Treatment Temp. 23.0 °C, Time 252000 sec |
|
Descriptive Properties |
---|
Color | Black |
TR-10 Temperature | -32.6°F |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.