MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carpenter Custom 450® Stainless Steel, Condition H900 (Age Hardened 482°C)
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Data provided by Carpenter Technology Corporation.

Custom 450® stainless is a martensitic age-hardenable stainless steel which exhibits very good corrosion resistance (similar to that of Stainless Type 304) with moderate strength (similar to that of Stainless Type 410). the alloy has a yield strength somewhat greater than 100 ksi (689 MPa) in the annealed condition, but is easily fabricated. A single-step aging treatment develops higher strength with good ductility and toughness. This stainless can be machined, hot-worked, and cold-formed in the same manner as other martensitic age-hardenable stainless steels. A particular advantage is ease of welding and brazing. Custom 450 stainless is generally supplied in the annealed condition, requiring no heat treatment by the user for many applications. Because it has corrosion resistance like Type 304 stainless but three times the yield strength, it has been used in applications where Type 304 was not strong enough. On the other hand, it has also replaced Type 410 stainless directly on a strength basis where Type 410 had insufficient corrosion resistance. Mechanical properties will depend on the aging temperature selected.

Custom 450® is a registered trademark of Carpenter Technology Corporation.

Key Words: UNS S45000
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.76 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 395Estimated from Rockwell C for 3000 kg load, 10 mm ball Brinell measurement.
Hardness, Knoop 431Estimated from Rockwell C
Hardness, Rockwell C 42.5
Hardness, Vickers 413Estimated from Rockwell C
Tensile Strength, Ultimate 1351 MPa
 579 MPa
@Temperature 566 °C
 1034 MPa
@Temperature 427 °C
 1103 MPa
@Temperature 316 °C
 1413 MPa
@Temperature -18.0 °C
 1489 MPa
@Temperature -73.0 °C
 1793 MPa
@Temperature -196 °C
Tensile Strength, Yield 1296 MPa
@Strain 0.2 %
 524 MPa
@Strain 0.2 %,
Temperature 566 °C
 903 MPa
@Strain 0.2 %,
Temperature 427 °C
 951 MPa
@Strain 0.2 %,
Temperature 316 °C
 1338 MPa
@Strain 0.2 %,
Temperature -18.0 °C
 1427 MPa
@Strain 0.2 %,
Temperature -73.0 °C
 1717 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 14 %In 4D
 5.0 %
@Temperature -196 °C
In 4D
 12 %
@Temperature 316 °C
In 4D
 12 %
@Temperature 427 °C
In 4D
 15 %
@Temperature -18.0 °C
In 4D
 16 %
@Temperature -73.0 °C
In 4D
 24 %
@Temperature 566 °C
In 4D
Reduction of Area 56 %
 8.0 %
@Temperature -196 °C
 45 %
@Temperature 427 °C
 48 %
@Temperature 316 °C
 57 %
@Temperature -18.0 °C
 75 %
@Temperature 566 °C
Modulus of Elasticity 200 GPa
Notched Tensile Strength 586 MPa
@Temperature -196 °C
Kt = 10
 1770 MPa
@Temperature -73.0 °C
Kt = 10
 2060 MPa
@Temperature 23.0 °C
Kt = 10
 2110 MPa
@Temperature -18.0 °C
Kt = 10
Poissons Ratio 0.29
Fatigue Strength 660 MPa
@# of Cycles 1.00e+7
R.R. Moore Test, Smooth Rotating Beam
Shear Modulus 77.5 GPaCalculated
Charpy Impact 54.0 JV-notch
 1.00 J
@Temperature -196 °C
V-notch
 5.00 J
@Temperature -73.0 °C
V-notch
 22.0 J
@Temperature -18.0 °C
V-notch
 57.0 J
@Temperature 427 °C
V-notch
 89.0 J
@Temperature 566 °C
V-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000846 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.8 µm/m-°C
@Temperature 24.0 - 93.0 °C
 10.87 µm/m-°C
@Temperature 24.0 - 260 °C
 11.75 µm/m-°C
@Temperature 24.0 - 593 °C
Specific Heat Capacity 0.477 J/g-°C
Thermal Conductivity 15.0 W/m-K
@Temperature 23.0 °C
condition H 900
 18.2 W/m-K
@Temperature 200 °C
condition H 900
 24.4 W/m-K
@Temperature 500 °C
condition H 900
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.050 %min. Nb content = 8 x C content
Chromium, Cr 14 - 16 %
Copper, Cu 1.25 - 1.75 %
Iron, Fe 75 %as remainder
Manganese, Mn <= 1.0 %
Molybdenum, Mo 0.50 - 1.0 %
Nickel, Ni 5.0 - 7.0 %
Phosphorus, P <= 0.030 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1010 Steel, cold drawn
ASTM A572 Steel, grade 50
AISI 1018 Steel, cold drawn
AISI 4140 Steel, normalized at 870°C (1600°F), reheated to 845°C (1550°F), oil quenched, 650°C (1200°F) temper, 25 mm (1 in.) round
AISI 4140 Steel, oil quenched, 25 mm (1 in.) round [845°C (1550°F) quench, 540°C (1000°F) temper]

NCAR84 / 15659

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.