MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Teknor Apex Telcar® TL-2550A Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Telcar TL-2550A is a general purpose, low density thermoplastic elastomer designed for injection molding applications.

Features: General Purpose; Good Colorability; High Flow; Low Density; Low Hardness; Low Specific Gravity; Oil Extended

Uses: General Purpose; Grommets; Industrial Applications; Industrial Parts

Form: Pellets

Processing Method: Injection Molding; Extrusion

Injection Notes: Injection Rate: Moderate-Fast

Extrusion Notes: Screw Speed: 30 to 100 rpm

Information Provided by Teknor Apex

Key Words: TPE
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.890 g/cc0.890 g/ccASTM D792
Melt Flow 21 g/10 min
@Load 2.16 kg,
Temperature 190 °C
21 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 4747ASTM D2240
Tensile Strength at Break 6.21 MPa900 psiASTM D412
Elongation at Break 800 %800 %ASTM D412
Tear Strength 20.2 kN/m115 pliAcross Flow; ASTM D624
 27.2 kN/m155 pliFlow; ASTM D624
Compression Set  20 %
@Temperature 22.8 °C,
Time 79200 sec
20 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 40 %
@Temperature 70.0 °C,
Time 79200 sec
40 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 171 - 193 °C340 - 380 °F
Middle Barrel Temperature 177 - 199 °C350 - 390 °F
Front Barrel Temperature 182 - 204 °C360 - 400 °F
Nozzle Temperature 188 - 210 °C370 - 410 °F
Zone 1 166 - 188 °C330 - 370 °F
Zone 2 171 - 193 °C340 - 380 °F
Zone 3 177 - 199 °C350 - 390 °F
Zone 5 182 - 204 °C360 - 400 °F
Die Temperature 190 - 210 °C374 - 410 °F
Melt Temperature 188 - 210 °C370 - 410 °FProcessing Temperature
Mold Temperature 25.0 - 65.6 °C77.0 - 150 °F
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Telcar® TL-2454A Thermoplastic Elastomer

PTEKNP456 / 129537

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.