MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Special Metals INCOLOY® A-286 Iron-Nickel-Chromium Alloy (UNS S66286)
Categories: Metal; Superalloy; Iron Base

Material Notes: An alloy that is precipitation hardenable for high mechanical properties. The alloy maintains good strength and oxidation resistance at temperatures up to about 1300°F (700°C). Its high strength and excellent fabrication characteristics make it useful for various components of aircraft and industrial gas turbines. Applications include blades, vanes, shafts, tail cones, afterburners, springs and fasteners, and automotive applications.

Tensile properties reported for Precipitation Hardened samples unless noted.

Data provided by the manufacturer, Special Metals.

Key Words: ASTM A 453, A 638
ASME SA-453, SA-638
SAE AMS 5525, 5726, 5731, 5732, 5734, 5737, 5858, 5895, 7235
BS HR 51, HR 52, HR 650
AECMA Pr EN 2119, 2171 – 2175, 2303, 2304, 2398, 2399, 2417, 3510
NACE MR-0175/ISO 15156
W. NR. 1.4980
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.94 g/cc0.287 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 3131As Annealed
Tensile Strength, Ultimate  517 MPa
@Temperature 760 °C
75000 psi
@Temperature 1400 °F
 689 MPa
@Temperature 649 °C
100000 psi
@Temperature 1200 °F
 862 MPa
@Temperature 538 °C
125000 psi
@Temperature 1000 °F
 931 MPa
@Temperature 427 °C
135000 psi
@Temperature 800 °F
 965 MPa
@Temperature 316 °C
140000 psi
@Temperature 600 °F
 1000 MPa
@Temperature 204 °C
145000 psi
@Temperature 400 °F
 1030 MPa
@Temperature 93.3 °C
150000 psi
@Temperature 200 °F
 1090 MPa
@Temperature 21.1 °C
158000 psi
@Temperature 70.0 °F
Tensile Strength, Yield  379 MPa
@Strain 0.2 %,
Temperature 760 °C
55000 psi
@Strain 0.2 %,
Temperature 1400 °F
 552 MPa
@Strain 0.2 %,
Temperature 649 °C
80000 psi
@Strain 0.2 %,
Temperature 1200 °F
 586 MPa
@Strain 0.2 %,
Temperature 538 °C
85000 psi
@Strain 0.2 %,
Temperature 1000 °F
 621 MPa
@Strain 0.2 %,
Temperature 427 °C
90000 psi
@Strain 0.2 %,
Temperature 800 °F
 655 MPa
@Strain 0.2 %,
Temperature 316 °C
95000 psi
@Strain 0.2 %,
Temperature 600 °F
 689 MPa
@Strain 0.2 %,
Temperature 204 °C
100000 psi
@Strain 0.2 %,
Temperature 400 °F
 724 MPa
@Strain 0.2 %,
Temperature 93.3 °C
105000 psi
@Strain 0.2 %,
Temperature 200 °F
 758 MPa
@Strain 0.2 %,
Temperature 21.1 °C
110000 psi
@Strain 0.2 %,
Temperature 70.0 °F
Elongation at Break  18 %
@Temperature 649 °C
18 %
@Temperature 1200 °F
 20 %
@Temperature 760 °C
20 %
@Temperature 1400 °F
 20 %
@Temperature 538 °C
20 %
@Temperature 1000 °F
 22 %
@Temperature 427 °C
22 %
@Temperature 800 °F
 24 %
@Temperature 316 °C
24 %
@Temperature 600 °F
 26 %
@Temperature 204 °C
26 %
@Temperature 400 °F
 28 %
@Temperature 93.3 °C
28 %
@Temperature 200 °F
 30 %
@Temperature 21.1 °C
30 %
@Temperature 70.0 °F
Modulus of Elasticity 201 GPa29200 ksiAs Annealed
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000910 ohm-cm0.0000910 ohm-cmAs Annealed
Magnetic Permeability 1.0071.007at 200 Oersted (15.9 kA/m)
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.4 µm/m-°C
@Temperature 27.0 - 100 °C
9.11 µin/in-°F
@Temperature 80.6 - 212 °F
Mean
 16.9 µm/m-°C
@Temperature 27.0 - 300 °C
9.39 µin/in-°F
@Temperature 80.6 - 572 °F
Mean
 17.5 µm/m-°C
@Temperature 27.0 - 500 °C
9.72 µin/in-°F
@Temperature 80.6 - 932 °F
Mean
 17.7 µm/m-°C
@Temperature 27.0 - 700 °C
9.83 µin/in-°F
@Temperature 80.6 - 1290 °F
Mean
Specific Heat Capacity 0.419 J/g-°C0.100 BTU/lb-°F
Thermal Conductivity 12.7 W/m-K88.1 BTU-in/hr-ft²-°FAs Annealed
Melting Point 1370 - 1430 °C2500 - 2610 °F
Solidus 1370 °C2500 °F
Liquidus 1430 °C2610 °F
Maximum Service Temperature, Air 700 °C1290 °Fgood strength and oxidation resistance
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.35 %<= 0.35 %
Boron, B 0.0010 - 0.010 %0.0010 - 0.010 %
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 13.5 - 16 %13.5 - 16 %
Iron, Fe 60 %60 %As remainder
Manganese, Mn <= 2.0 %<= 2.0 %
Molybdenum, Mo 1.0 - 1.5 %1.0 - 1.5 %
Nickel, Ni 24 - 27 %24 - 27 %
Sulfur, S <= 0.030 %<= 0.030 %
Titanium, Ti 1.9 - 2.35 %1.9 - 2.35 %
Tungsten, W 3.0 - 4.5 %3.0 - 4.5 %
Vanadium, V 0.10 - 0.50 %0.10 - 0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® Nickelvac® A-286 Specialty Steel, Heat Treatment: 982°C (1800°F) + Age
ATI Allegheny Ludlum Altemp® A286 Iron-Base Superalloy, UNS S66286
Aperam Superimphy® 286 Bar-Corrosion application
A286 IRON BASED 15Cr-26Ni-1.3Mo-2.1Ti-0.3V SUPERALLOY FORGINGS FOR GAS TURBINE DISCS
660 Stainless Steel (A286) short time tensile test

NINCO01 / 17434

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.