System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Envalior Stanyl® TS250F6D PA46-GF30 FR, Dry, 30% Glass Filled, Flame Retardant, Heat Stabilized
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 46 (PA46)
;
Nylon 46, Flame Retarded + Glass Fiber Reinforced
Material Notes:
30% Glass Reinforced, Flame Retardant, Heat Stabilized, Improved resistance to blistering during reflow-soldering process
Former DSM Engineering Plastics product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.68
g/cc
ISO 1183
Moisture Absorption
1.50 %
Humidity; Sim. ISO 62
Linear Mold Shrinkage, Flow
0.0040
cm/cm
ISO 294-4
Linear Mold Shrinkage, Transverse
0.011
cm/cm
ISO 294-4
Mechanical Properties
Original Value
Comments
Tensile Strength at Break
180
MPa
ISO 527-1/-2
Elongation at Break
2.5 %
ISO 527-1/-2
Tensile Modulus
12000
MPa
ISO 527-1/-2
Flexural Modulus
11000
MPa
ISO 178
Izod Impact, Notched (ISO)
11.0
kJ/m²
@Temperature 23.0 °C
ISO 180/1A
11.0
kJ/m²
@Temperature -40.0 °C
ISO 180/1A
Charpy Impact Unnotched
50.0
kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
60.0
kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched
10.0
kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
11.0
kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
Electrical Properties
Original Value
Comments
Volume Resistivity
>=
1.00e+13
ohm-cm
IEC 60093
Dielectric Strength
30.0
kV/mm
IEC 60243-1
Comparative Tracking Index
250
V
IEC 60112
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
25.0
µm/m-°C
ISO 11359-1/-2
CTE, linear, Transverse to Flow
55.0
µm/m-°C
ISO 11359-1/-2
Melting Point
295
°C
10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi)
290
°C
ISO 72-1/-2
Flammability, UL94
V-0
@Thickness 1.50 mm
IEC 60695-11-10
V-0
@Thickness 0.670 mm
IEC 60695-11-10
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Celanese Zytel® HTN51G35HSL NC010 PA6T/XT-GF35
Celanese FORTRON 1140L6 PPS, 40% Glass Reinforced
Celanese Zenite® 6130 BK010 LCP, 30% glass reinforced (Extended Tabular Temperature Data)
Celanese Thermx® CG933 NC010 PCT
DSM Stanyl® ForTii™ F11C PA4T-GF30 FR (40), Dry, 30% Glass Filled, Flame Retardant
PDSM8227 / 184928
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.