MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Teknor Apex APEX® RE 8003 Polyvinyl Chloride, Rigid
Categories: Polymer; Thermoplastic; Vinyl (PVC); PVC, High Impact; PVC, Rigid Grade

Material Notes: Features: High Impact Resistance; Medium Gloss

Processing Method: Extrusion

Forms: Pellets

Additional Information: Performance Characteristics: Yellow Card, Interior, Medium Gloss, Excellent Finish

Information Provided by Teknor Apex

Key Words: PVC
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.44 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 8010 seconds; ASTM D2240
Tensile Strength at Break 6510 psiASTM D638
Tensile Strength, Yield 6520 psiASTM D638
Elongation at Break 54 %ASTM D638
Elongation at Yield 3.1 %ASTM D638
Tensile Modulus 345000 psiASTM D638
Flexural Modulus 389000 psiASTM D790
Izod Impact, Notched 14.0 ft-lb/in
@Thickness 3.17 mm,
Temperature 22.8 °C
Compression Molded; ASTM D256
Dart Drop Total Energy 0.192 ft-lb/mil
@Thickness 3.17 mm,
Temperature 22.8 °C
Procedure B, 0.250" Conical Dart; ASTM D4226
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 157 °F
@Thickness 3.17 mm
Annealed; ASTM D648
Flammability, UL94 5VA
 V-0
@Thickness 22.9 mm
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Arkema Nakan® RMA 705 N PVC, Rigid Injection Molding Grade
Arkema Nakan® RMS 501 L PVC, Rigid Injection Molding Grade
Karina 802-18/462-C-ERB Gray PVC Compound
Teknor Apex Sinvicomp SRF 3703 Polyvinyl Chloride, Rigid
AlphaGary Dural 725C CLEAR 0003 Full Rigid Polyvinyl Chloride Compound

PTEKNO689 / 128867

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.