Polyram RamLloy PA917G4 PP/NYLON 66 alloy, 20% Glass Fiber
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Polypropylene (PP)
Material Notes:
20% glass fiber reinforced PA66/PP alloy with reduced water absorption, dimensional stability and UV stabilized for injection molding applications
Information provided by Polyram Ram On Ind.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.21
g/cc
0.0437
lb/in³
DIN 53479
Water Absorption
3.5 %
3.5 %
DIN 53495
Moisture Absorption at Equilibrium
1.5 %
1.5 %
DIN 53714
Linear Mold Shrinkage
0.00
-
0.0050
cm/cm
0.00
-
0.0050
in/in
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
121
121
ASTM-D785
Tensile Strength, Yield
115
MPa
16700
psi
ASTM-D638
Elongation at Break
3.0 %
3.0 %
ASTM-D638
Flexural Strength
195
MPa
28300
psi
ASTM-D790
Flexural Modulus
5.70
GPa
827
ksi
ASTM-D790
Izod Impact, Notched
1.00
J/cm
@Temperature 23.0 °C
1.87
ft-lb/in
@Temperature 73.4 °F
ASTM-D256
Thermal Properties
Metric
English
Comments
Melting Point
256
°C
493
°F
Maximum Service Temperature, Air
80.0
°C
176
°F
Continuous Use
150
°C
302
°F
Short peaks operation
Flammability, UL94
HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
EPICHEM Epilen PP 20GF NAT Polypropylene, 20% Glass Fiber
Premix Thermoplastics PREBLACK PP 704-35 Polypropylene, 35% Carbon Black
Polyram RamLloy PB917G6 Nylon 6/Polypropylene Alloy, 30% Glass Fiber Reinforced
Kuraray Genestar™ GC1201A-M41 Nylon, Glass Filled and Carbon Filled
NCMT NanoPAC™ G1550S High Performance Polypropylene Nanocomposite
PPOLYRA354 / 57616
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.