MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LyondellBasell Plexar® PX3410 Extrudable Tie-Layer Resin - Anhydride Modified LLDPE  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Anhydride-Modified Polyethylene; Linear Low Density (LLDPE)

Material Notes: Applications
Plexar® tie-layers are chemically modified resins used to bond unlike materials, primarily in packaging and industrial applications. Common adherents include polyethylene resins and copolymers, such as EVA or EMA, polypropylene, polyamide (nylon), ethylene vinyl alcohol copolymers (EVOH), ionomer and other sealants, polyethylene terephthalate (PET) resins and copolymers, styrenic polymers, metal, paper and many others. Product grades tailored for blown and cast films, sheet and thermoforming, blow molding, extrusion coating and lamination, tubing, pipe, spray coating and other specialty applications are available in pellet form.

Regulatory Status
Plexar tie-layers meet the requirements for the Food and Drug Administration regulation 21CFR 175.105 for adhesives. This regulation describes adhesives which may be safely used as components of articles intended for use in packaging, transporting or holding food in accordance with conditions outlined in that regulation. For an adhesive formulation to be used in compliance with Section 175.105, it must be used under conditions that prevent the material from becoming a component of food in more than insignificant, de minimis, amounts.

Processing
A process melt temperature above 410°F (210°C) is recommended to ensure adhesion between adherents. More specific suggestions can be made only when equipment, process parameters and conditions of use are known.

This product is from the former Equistar product line.

Key Words: Linear Low Density Polyethylene
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.915 g/ccASTM D1505
Water Vapor Transmission 9.07 g/m²/day100% Humidity; ASTM F372
Thickness 2.00 mil
Melt Flow 1.0 g/10 min
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 10.8 MPaASTM D882
Film Tensile Strength at Yield, TD 12.7 MPaASTM D882
Film Elongation at Break, MD 650 %ASTM D882
Film Elongation at Break, TD 710 %ASTM D882
Film Elongation at Yield, MD 8.0 %ASTM D882
Film Elongation at Yield, TD 10 %ASTM D882
Elmendorf Tear Strength MD 640 gNotched; ASTM D1922
Elmendorf Tear Strength TD 1100 gNotched; ASTM D1922
Elmendorf Tear Strength, MD 320 g/milbased on 2 mil film; ASTM D1922
Elmendorf Tear Strength, TD 550 g/milbased on 2 mil film; ASTM D1922
Film Tensile Strength at Break, MD 52.1 MPaASTM D882
Film Tensile Strength at Break, TD 40.0 MPaASTM D882
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 102 °CASTM D1525
 
Processing PropertiesOriginal ValueComments
Melt Temperature >= 410 °F
 
Compliance PropertiesOriginal ValueComments
FDA Yes

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dymax 3073 Solvent-Free Plastic Adhesive
Dow Bynel® 30E753 Anhydride Modified Ethylene Vinyl Acetate
ExxonMobil LD 145.PX Packaging Resin
Covestro Bayhydrol® A 145 Polyurethane Coating
LyondellBasell Plexar® PX5125 Extrudable Tie-Layer Resin - Anhydride Modified LLDPE

PEQU0704 / 37173

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.