MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Oxford Polymers 40GF 40% Glass Fiber Filled Polyetherimide for Extrusion and Injection Molding
Categories: Polymer; Thermoplastic; Polyetherimide (PEI); Polyetherimide (PEI), 40% Glass Fiber

Material Notes: 40% Glass Fiber Filled Polyetherimide for Extrusion and Injection Molding

Information provided by Oxford Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.60 g/ccASTM D792
Filler Content 40 %
Water Absorption 0.13 %ASTM D570
Linear Mold Shrinkage 0.0020 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 26000 psiASTM D638
Elongation at Break 2.0 %ASTM D638
Tensile Modulus 1.50e+6 psiASTM D638
Flexural Strength 34.0 ksiASTM D790
Flexural Modulus 1600 ksiASTM D790
Izod Impact, Notched 1.80 ft-lb/in
@Temperature 23.0 °C
ASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 415 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 410 °FASTM D648
 
Processing PropertiesOriginal ValueComments
Processing Temperature 720 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled
Overview of materials for Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler
Celanese VECTRA® H140 40% Glass Filled Liquid Crystal Polymer (LCP)
Oxford Polymers 10GF 10% Glass Fiber Filled Polyetherimide for Extrusion and Injection Molding
Oxford Polymers 20GF 20% Glass Fiber Filled Polyetherimide for Extrusion and Injection Molding

POX19 / 55868

Ensinger SPI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.