MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Monprene® OM-10160 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene OM-10160 is a high performance thermoplastic elastomer designed for overmolding applications like grips and anti-skid parts for a variety of consumer products. Monprene OM-10160 is a medium hardness, low density opaque grade that exhibits excellent adhesion to nylon.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Abrasion Resistant; Bondability; Chemical Resistant; Good Adhesion; Good Colorability; ;Good Flexibility; Good Moldability; Good Processability; Good Surface Finish; Good Tear Strength; Good Toughness; Halogen Free; Low Density; Low Specific Gravity; Medium Hardness; Resilient

Uses: Appliances; Bonding; Cell Phones; Consumer Applications; Flexible Grips; Handles; Knobs; Luggage; Overmolding; Plugs; Power/Other Tools; Rubber Replacement; Soft Touch Applications; Sporting Goods; White Goods & Small Appliances

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³ASTM D792
Melt Flow 15 g/10 min
@Load 2.16 kg,
Temperature 190 °C
15 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6262ASTM D2240
 60
@Time 5.00 sec
60
@Time 0.00139 hour
ASTM D2240
Tensile Strength at Break 5.52 MPa800 psiASTM D412
Elongation at Break 600 %600 %ASTM D412
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 204 - 232 °C400 - 450 °F
Middle Barrel Temperature 210 - 232 °C410 - 450 °F
Front Barrel Temperature 216 - 238 °C420 - 460 °F
Nozzle Temperature 221 - 243 °C430 - 470 °F
Melt Temperature 221 - 243 °C430 - 470 °F
Mold Temperature 23.9 - 60.0 °C75.0 - 140 °F
Drying Temperature 65.6 °C150 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.862 MPa25.0 - 125 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 120 rpm50 - 120 rpm
 
Descriptive Properties
AppearanceBlack
 Colors Available
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ0888 / 237379

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.