MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

SABIC LNP™ LUBRICOMP™ Compound OCL36 Polyphenylene Sulfide, Linear (PPS, Linear) (Asia)
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes: LNP LUBRICOMP OCL36 compound is based on Polyphenylene Sulfide (PPS) - linear resin containing 30% carbon fiber and 15% PTFE. Added features of this grade include: Electrically Conductive, Wear Resistant.

Features: Light-weight Structural,Super Strong (Carbon Fiber Filled),Wear resistant,Electrically Conductive,Structural

Information provided by SABIC

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.52 g/cc0.0549 lb/in³ASTM D792
 1.52 g/cc0.0549 lb/in³ISO 1183
Moisture Absorption 0.0300 %0.0300 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0020 - 0.0040 cm/cm0.0020 - 0.0040 in/in24hrs; ASTM D955
 0.0020 - 0.0040 cm/cm0.0020 - 0.0040 in/in24hrs; ISO 294
Linear Mold Shrinkage, Transverse 0.0030 - 0.0040 cm/cm0.0030 - 0.0040 in/in24hrs; ASTM D955
 0.0036 - 0.0040 cm/cm0.0036 - 0.0040 in/in24hrs; ISO 294
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 166 MPa24100 psiISO 527
 168 MPa24400 psiASTM D638
Elongation at Break 1.1 %1.1 %ISO 527
 1.4 %1.4 %ASTM D638
Tensile Modulus 21.51 GPa3120 ksi5 mm/min; ASTM D638
 30.68 GPa4450 ksi1 mm/min; ISO 527
Flexural Strength 259 MPa37600 psiASTM D790
 262 MPa38000 psiISO 178
Flexural Modulus 21.11 GPa3062 ksiASTM D790
 21.2 GPa3070 ksiISO 178
Izod Impact Notched 58.0 J42.8 ft-lbASTM D256
Izod Impact, Unnotched 4.43 J/cm8.30 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 6.00 kJ/m²2.86 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 31.0 kJ/m²14.8 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 15.0 J11.1 ft-lbpeak; ASTM D3763
Impact Test 2.00 J1.48 ft-lbMultiaxial Impact; ISO 6603
Coefficient of Friction, Dynamic 0.390.39ASTM D3702 Modified: Manual
Coefficient of Friction, Static 0.340.34ASTM D3702 Modified: Manual
K (wear) Factor 38.3 x 10-8 mm³/N-M19.0 x 10-10 in³-min/ft-lb-hrWasher; ASTM D3702 Modified: Manual
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 263 °C505 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 267 °C
@Thickness 3.20 mm
513 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 320 - 330 °C608 - 626 °F
Zone 3 330 - 345 °C626 - 653 °F
Melt Temperature 315 - 320 °C599 - 608 °FInjection Molding
Mold Temperature 140 - 165 °C284 - 329 °F
Drying Temperature 120 - 150 °C248 - 302 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80911 / 288858

Ensinger SPI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.