MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SEKISUI SPI KYDEX® 5555HI Thermoplastic sheet
Categories: Polymer; Thermoplastic

Material Notes: KYDEX® 5555HI is a proprietary, high performance thermoplastic sheet with integral color specifically engineered to improve aircraft passenger safety.

KYDEX® 5555HI is designed to provide material deformation when used in components subjected to HIC (Head Injury Criterion) testing for increased passenger safety. It exceeds the flammability and smoke development requirements outlined in Federal Aviation Regulations (FAR) 25.853 paragraphs (a) and (d). KYDEX® 5555HI exceeds a 55/55 heat release level and 150 smoke development that allows the product to be used as a stand-alone material or within bonded build-up constructions.

Suggested Application:

  • Seat parts
  • Bulkhead laminates
  • Life vest shrouds
  • Passenger service units
  • Monitor Shrouds
  • Armrests
  • Molding strips
  • Tray tables
  • Kick panels
  • Bonded build-ups
Features:
  • Improved impact properties over traditional thermoplastics for HIC compliance seating requirements
  • Reduces cost of compliance by decreasing the total number of expensive and time consuming 16g tests required
  • Increases design freedom to create more complex seat geometries
  • Decreases weight by eliminating the need for heavy reinforcements or thick gauges
  • Exceeds the stringent requirements of FAR 25.853 paragraphs (a) and (d) in all thicknesses and colors, which allows for bonded build-up constructions
  • Excellent formability and fabrication characteristics
  • Processes similar to KYDEX® 5555
  • Allows for tight tolerance control
  • Available in a wide range of integral colors

Information provided by SEKISUI KYDEX, LLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.48 g/cc1.48 g/ccASTM D792
Water Absorption 0.0800 %
@Time 86400 sec
0.0800 %
@Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 106106ASTM D785
Tensile Strength 45.1 MPa6540 psiASTM D638
Tensile Modulus 3.261 GPa473.0 ksiASTM D638
Flexural Strength 71.7 MPa10400 psiASTM D790
Flexural Modulus 3.15 GPa457 ksiASTM D790
Compressive Yield Strength 58.3 MPa8460 psiASTM D695
Compressive Modulus 1.958 GPa284.0 ksiASTM D695
Bearing Yield Strength <= 207.5 MPa<= 30100 psiASTM D953
 32.2 MPa
@Strain 4.00 %
4670 psi
@Strain 4.00 %
ASTM D953
Poissons Ratio 0.3850.385ASTM D638
Shear Strength 48.5 MPa7030 psiASTM D732
Gardner Impact 62.9 J46.4 ft-lbDrop Dart Impact, GE; ASTM D5420
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 19.7 kV/mm500 kV/inoil; ASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear 34.2 µm/m-°C19.0 µin/in-°FASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 76.9 °C170 °Fannealed; ASTM D648
Smoke Density <= 150<= 150FAR 25.853(d) Part V
 
Descriptive Properties
OSU Heat Release<55/55 kW/m2FAR 25.853(d) Part IV
Vertical BurnPass60 and 12 sec; FAR 25.853(a)(i) and FAR 25.853(a)(ii)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSEKIS519 / 325259

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.