MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Saint-Gobain Spectrosil® 2000 Optical Fused Quartz
Categories: Ceramic; Glass; Oxide; Silicon Oxide

Material Notes: Spectrosil® 2000 is a deep UV, fluorescence-free grade.

Spectrosil® is a synthetic fused silica manufactured using a patented, environmentally friendly process that results in a virtually chlorine-free material of exceptional purity which is bubble-free and fluorescence-free. The 2000 series has excellent optical transmission from 180 nm in the deep UV through to 2000 nm in the IR Available in ingot, rod, tube, and components.

General properties of Fused Silica and Fused quartz: A very wide transmission range from UV to near IR; extremely high optical transmission, excellent resistance to high power laser energy, excellent homogeneity, high temperature resistance, very low thermal expansion (resistance to thermal shock), and chemical inertness. General uses for optical quartz are microlithography optical systems, optical fibers, photomasks, laser optics, LCD displays, light guides, optical, IR , and UV windows, spectrophotometer cells, slides, optical pyrometers, and lamp bodies/components.

Information provided by Saint-Gobain Quartz PLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.21 g/cc0.0798 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 820820
Vickers Microhardness 1050 - 13501050 - 1350kg/m² Vickers DPH
Hardness, Mohs 7.07.0
Modulus of Elasticity 74.0 GPa10700 ksi
Flexural Strength 50.0 MPa7250 psiBending Strength
Compressive Strength 1100 MPa160000 psi
Poissons Ratio 0.170.17
Shear Modulus 31.0 GPa4500 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 2.00e+10 ohm-cm
@Temperature 800 °C
2.00e+10 ohm-cm
@Temperature 1470 °F
Dielectric Constant 3.78
@Frequency 100 - 2.50e+10 Hz
3.78
@Frequency 100 - 2.50e+10 Hz
Dissipation Factor  0.000060
@Frequency 1e+9 Hz
0.000060
@Frequency 1e+9 Hz
 0.00075
@Frequency 1000 Hz
0.00075
@Frequency 1000 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear 0.540 µm/m-°C
@Temperature 0.000 - 1000 °C
0.300 µin/in-°F
@Temperature 32.0 - 1830 °F
average
Specific Heat Capacity 0.750 J/g-°C0.179 BTU/lb-°F
Thermal Conductivity 2.00 W/m-K13.9 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 1050 °C1920 °FNormal Conditions
 1350 °C2460 °FExtended periods if cycles remain above 300°C
 1350 °C2460 °F
 1650 °C3000 °FQuick Immersion
Softening Point 1710 °C3110 °FVaries with thermal history
Annealing Point 1100 °C2010 °FVaries with thermal history
Strain Point 990 °C1810 °FVaries with thermal history
 
Optical PropertiesMetricEnglishComments
Refractive Index  1.457
@Wavelength 632.8 nm
1.457
@Wavelength 632.8 nm
nHe-Ne; Temperature Coefficient = 10.0 ppm/K
 1.4667
@Wavelength 435.83 nm
1.4667
@Wavelength 435.83 nm
ng; Temperature Coefficient = 10.6 ppm/K
Transmission, Visible 95 %95 %Including Fresnel reflection for 10 mm pathlength
IR Transmittance 95 %
@Wavelength <=2000 nm,
Thickness 10.0 mm
95 %
@Wavelength <=2000 nm,
Thickness 0.394 in
Including Fresnel reflection for 10 mm path length.
UV Transmittance  >= 99.5 %
@Thickness 10.0 mm,
Wavelength 193.4 nm
>= 99.5 %
@Thickness 0.394 in,
Wavelength 193.4 nm
 >= 99.9 %
@Thickness 10.0 mm,
Wavelength 240 nm
>= 99.9 %
@Thickness 0.394 in,
Wavelength 240 nm
 
Component Elements PropertiesMetricEnglishComments
SiO2 >= 99.999 %>= 99.999 %
 
Descriptive Properties
Bubble Class0per DIN 58927
Bubbles; Sum of CSA< 0.03 mm²/100 cm³
Inclusions0
Refractive Index Homogeneity< 25 x 10-6Up to 200 mm (ingot)
Residual Strain<10 nm/cmexcept edge
Striae1per MIL-G-174A; Direction Free

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Saint-Gobain Spectrosil® 2200 Optical Fused Quartz
Corning Willow® Flexible Display Glass
Ohara BSM51Y i-Line Optical Glass
Schott N-F2 Glass
Schott N-LAF33 Glass

CSTGQZ02 / 2220

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.