MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC LNP™ LUBRICOMP™ Compound RFL36 Polyamide 66 (Nylon 66)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: LNP LUBRICOMP RFL36 compound is based on Nylon 6/6 resin containing 30% glass fiber, 15% PTFE. Added features of this grade include: Wear Resistant.

Features: Wear resistant,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.51 g/ccISO 1183
Water Absorption 1.34 %
@Time 86400 sec
ISO 62-1
Moisture Absorption 0.150 - 0.250 %Injection Molding
 0.460 %23°C / 50% RH; ISO 62
Viscosity 15 - 20 cP
@Load 5.00 kg,
Temperature 275 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0020 - 0.0050 cm/cm24hrs; ISO 294
Linear Mold Shrinkage, Transverse 0.0080 - 0.012 cm/cm24hrs; ISO 294
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 166 MPa5 mm/min; ISO 527
Elongation at Break 2.6 %5 mm/min; ISO 527
Flexural Strength 234 MPayield, 2 mm/min; ISO 178
 277 MPabreak, 2mm/min; ISO 178
 83.0 MPa
@Temperature 200 °C
yield, 2 mm/min; ISO 178
 96.0 MPa
@Temperature 150 °C
yield, 2 mm/min; ISO 178
 131 MPa
@Temperature 100 °C
yield, 2 mm/min; ISO 178
 179 MPa
@Temperature 60.0 °C
yield, 2 mm/min; ISO 178
Flexural Modulus 9100 MPa2 mm/min; ISO 178
 3100 MPa
@Temperature 200 °C
2 mm/min; ISO 178
 3500 MPa
@Temperature 150 °C
2 mm/min; ISO 178
 4200 MPa
@Temperature 100 °C
2 mm/min; ISO 178
 5300 MPa
@Temperature 60.0 °C
2 mm/min; ISO 178
Flexural Strain at Break 4.1 %2 mm/min; ISO 178
 5.6 %
@Temperature 150 °C
2 mm/min; ISO 178
 6.1 %
@Temperature 60.0 °C
2 mm/min; ISO 178
 6.3 %
@Temperature 200 °C
2 mm/min; ISO 178
 6.6 %
@Temperature 100 °C
2 mm/min; ISO 178
Izod Impact, Notched (ISO) 16.0 kJ/m²80*10*4; ISO 180/1A
 12.0 kJ/m²
@Temperature -40.0 °C
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) 84.0 kJ/m²80*10*4; ISO 180/1U
 74.0 kJ/m²
@Temperature -40.0 °C
80*10*4; ISO 180/1U
Coefficient of Friction, Dynamic 0.59ASTM D3702 Modified: Manual
K (wear) Factor 12.0 x 10-10 in³-min/ft-lb-hrWasher; ASTM D3702 Modified: Manual
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 25.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 75.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
Specific Heat Capacity 1.988 J/g-°CASTM E1269
Thermal Conductivity 0.250 W/m-KASTM D5930
Deflection Temperature at 0.46 MPa (66 psi) >= 220 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi) >= 220 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
UL RTI, Electrical 120 °CUL 746B
UL RTI, Mechanical with Impact 65.0 °CUL 746B
UL RTI, Mechanical without Impact 65.0 °CUL 746B
Flammability, UL94 HB
@Thickness >=0.750 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Zone 2 280 - 295 °C
Zone 3 295 - 305 °C
Melt Temperature 280 - 305 °CInjection Molding
Mold Temperature 95.0 - 110 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80986 / 288933

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.